Materials Supply / Copper & Copper-Base Alloys
C17200 Beryllium Copper (Alloy 25)
Alloy 25 | UNS C17200 | CuBe2 CW101C
C17200 contains 1.80–2.00% beryllium and reaches the highest strength of the copper alloys listed after ageing at 315°C.
It is not a high-conductivity grade: aged conductivity is about half that of C17500 or C17510.
Imagery is illustrative metal product forms, not certified C17200 stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
Materion lists strip, rod, tube, wire, bar, plate, forgings and extrusions. Confirm forms, sizes and availability at enquiry.
- Strip, sheet and plate
- Rod and bar
- Tube
- Wire
- Forgings and extrusions
Material overview
C17200 Beryllium Copper (Alloy 25)
The high-strength beryllium copper: age-hardens to around 1.2–1.4 GPa tensile strength with about 22% IACS conductivity.
- Flat and rod properties are separate conditions for each temper; mill-hardened strip is shown separately.
- Beryllium-containing: dust and fume from processing require exposure controls.
Designations and specifications
| Designation / standard | Scope and qualification |
|---|---|
| UNS / EN | C17200; CuBe2, CW101C (NGK) |
| Producer names | Materion Alloy 25; mill-hardened Alloy 190 / 290 |
| ASTM B194 | Plate, sheet, strip and rolled bar |
| ASTM B196/B196M | Rod and bar (confirms TB00/TD04/TF00/TH04 tempers) |
| ASTM B197/B197M | Wire |
| ASTM B570 | Forgings and extrusions |
| AMS4530 | TB00 sheet, strip and plate |
| AMS4533 | TF00 bar and rod — retrieved revision page is work in progress |
| AMS4532 / 4650 / 4651 / 4725; EN | Alloy and temper mappings not verified |
ASTM B196/B196M-24 — official listing
Specification review
Technical verification requirements
Physical
Materion aged plate reports 105 W/(m·K), 17.5 × 10⁻⁶/K (20–200°C), 131 GPa and 25–30% IACS, differing from CDA.
Use producer data for the ordered form.
Specifications
AMS4532/4650/4651/4725, RWMA and EN mappings unverified; AMS4533 revision is work in progress.
Obtain controlled standards.
Grade selection
C17200, C17500 and C17510 — strength versus conductivity
| Aspect | C17200 (Alloy 25) | C17500 (Alloy 10) | C17510 (Alloy 3) |
|---|---|---|---|
| Family | High-strength | High-conductivity | High-conductivity |
| Beryllium (CDA limits) | 1.80–2.00% | 0.40–0.70% | 0.20–0.60% |
| Main addition | Ni+Co ≥0.20% | Co 2.40–2.70% | Ni 1.40–2.20% |
| Peak-aged flat UTS (CDA) | 175–200 ksi typical (TF00–TH04) | 100–110 ksi minimum (TF00–TH04) | 110–115 ksi typical (TF00–TH04) |
| Conductivity, aged (CDA, 20°C) | 22% IACS | 45–48% IACS | 45% (AT) / 48% (HT) IACS |
| Ageing (Materion) | 315°C | 480°C | 480°C |
C17200 is not interchangeable with C17500 or C17510: it trades conductivity for strength. C17500 flat values are CDA minima; C17200 and C17510 are typical.
Copper Development Association — C17200 alloy record
Engineering reference
Technical data
| Element | Mass % |
|---|---|
| Beryllium | 1.80–2.00 |
| Nickel + cobalt | 0.20 min |
| Nickel + cobalt + iron | 0.60 max |
| Aluminium | 0.20 max |
| Silicon | 0.20 max |
| Copper (incl. Ag) | Remainder |
| Cu + named elements | 99.5 min |
No separate lead limit in the CDA entry; none is invented. NGK wire additionally limits Co ≤0.30%.
Copper Development Association — C17200 alloy record
| Property | CDA value | Basis |
|---|---|---|
| Electrical conductivity | 22% IACS | 20°C; precipitation hardened; form not stated |
| Thermal conductivity | 107–130 W/(m·K) (62–75 Btu/h·ft·°F) | 20°C; condition not stated |
| Density | 8.03 g/cm³ (0.290 lb/in³) | 20°C |
| Mean CTE | 17.8 × 10⁻⁶/K (9.9 × 10⁻⁶/°F), mean 20–300°C | Condition not stated |
| Elastic modulus (tension) | 128 GPa (18,500 ksi) | Temperature and temper not stated |
Metric figures converted from CDA customary units. Conductivity of solution-annealed (TB00) and cold-worked (TD04) material is not verified and is not assumed equal to the aged value.
Copper Development Association — C17200 alloy record
TB00 (A) solution annealed — flat products
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 70 ksi (483 MPa) | Typical |
| Yield strength (0.2% offset) | 32 ksi (221 MPa) | Typical |
| Elongation | 45% | Typical |
| Hardness | HRB 60 | Typical |
CDA values at 20°C for 0.188-in (4.8 mm) section flat products (TB00 thickness not stated). Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TD04 (H) solution annealed + hard — flat products
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 110 ksi (758 MPa) | Typical |
| Yield strength (0.2% offset) | 104 ksi (717 MPa) | Typical |
| Elongation | 5% | Typical |
| Hardness | HRB 99 | Typical |
CDA values at 20°C for 0.188-in (4.8 mm) section flat products (TB00 thickness not stated). Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TF00 (AT) solution annealed + aged — flat products
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 175 ksi (1207 MPa) | Typical |
| Yield strength (0.2% offset) | 155 ksi (1069 MPa) | Typical |
| Elongation | 6% | Typical |
| Hardness | HRC 38 | Typical |
CDA values at 20°C for 0.188-in (4.8 mm) section flat products (TB00 thickness not stated). Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TH04 (HT) hard + aged — flat products
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 200 ksi (1379 MPa) | Typical |
| Yield strength (0.2% offset) | 180 ksi (1241 MPa) | Typical |
| Elongation | 2% | Typical |
| Hardness | HRC 42 | Typical |
CDA values at 20°C for 0.188-in (4.8 mm) section flat products (TB00 thickness not stated). Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TB00 (A) solution annealed — rod
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 72 ksi (496 MPa) | Typical |
| Yield strength (0.2% offset) | 20 ksi (138 MPa) | Typical |
| Elongation | 20% | Typical |
| Hardness | HRB 65 | Typical |
CDA values at 20°C for rod, size not stated. Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TD04 (H) solution annealed + hard — rod
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 110 ksi (758 MPa) | Typical |
| Yield strength (0.2% offset) | 75 ksi (517 MPa) | Typical |
| Elongation | 8% | Typical |
| Hardness | HRB 95 | Typical |
CDA values at 20°C for 0.375-in (9.5 mm) rod. Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TF00 (AT) solution annealed + aged — rod
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 182 ksi (1255 MPa) | Typical |
| Yield strength (0.2% offset) | 130 ksi (896 MPa) | Typical |
| Elongation | 3% | Typical |
| Hardness | HRC 39 | Typical |
CDA values at 20°C for 3-in (76 mm) rod. Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TH04 (HT) hard + aged — rod
| Property | CDA value | Basis |
|---|---|---|
| Tensile strength | 195 ksi (1345 MPa) | Typical |
| Yield strength (0.2% offset) | 145 ksi (1000 MPa) | Typical |
| Elongation | 4% | Typical |
| Hardness | HRC 41 | Typical |
CDA values at 20°C for 3-in (76 mm) rod. Not interchangeable with other forms or tempers.
Copper Development Association — C17200 alloy record
TM02–TM08 mill hardened — flat products
| Temper | Tensile strength | 0.2% yield | Elongation | Hardness |
|---|---|---|---|---|
| TM02 | 128 ksi (883 MPa) | 105 ksi (724 MPa) | 15% | HRC 27 |
| TM04 | 142 ksi (979 MPa) | 122 ksi (841 MPa) | 12% | HRC 32 |
| TM06 | 168 ksi (1158 MPa) | 148 ksi (1020 MPa) | 7% | HRC 37 |
| TM08 | 182 ksi (1255 MPa) | 160 ksi (1103 MPa) | 6% | Not reported |
CDA typical values at 20°C. Individual TM conductivity not verified.
Copper Development Association — C17200 alloy record
Age hardening (Materion)
315°C — 2 h for cold-worked, 3 h for solution-annealed material.
Solution annealing (Materion)
790°C, then immediately water quench. Supplied wrought material is already solution annealed; unnecessary re-solution treatment risks distortion, grain growth and hazardous surface oxides.
Mill-hardened (TM) tempers
Supplied already age-hardened by the mill; no further customer ageing is normally required.
Exposure control
Heat treatment that forms oxide scale, and subsequent cleaning, requires beryllium exposure controls.
Soak times are counted after parts reach temperature. Materion guidance, not a complete qualified furnace recipe; CDA heat-treatment entries with ambiguous minute-based times are not used.
Typical applications
Engineering applications
- Connector and socket contacts
- Aerospace bushings and bearings
- Drilling-tool components
- Springs and wear parts
Subsequent manufacturing
Machining & processing
Beryllium health and safety
Beryllium-containing material: machining, grinding, polishing, welding and oxide-forming heat treatment can release beryllium dust, fume or coolant mist. Inhalation can cause sensitisation, chronic beryllium disease and cancer (Materion SDS). Solid, unprocessed parts present a different exposure situation, but this is not unconditional safety. Use engineering controls, extraction, hygiene and exposure monitoring. UK HSE EH40 lists a workplace exposure limit of 0.002 mg/m³ (2 µg/m³) 8-h TWA as Be, carcinogen — exposure must be kept as low as reasonably practicable. US OSHA: PEL 0.2 µg/m³ 8-h TWA; STEL 2.0 µg/m³; action level 0.1 µg/m³.
Machining
Machine with flood coolant and extraction; capture swarf, mist and dust. Normally machined before ageing, or in mill-hardened tempers.
Application evidence
Listed applications are producer-cited categories, not claims of stock or component approval.
Material certification & testing
Documentation must be agreed for the actual UNS/EN grade, product specification, form, temper and any conductivity or oxygen-content test.
No certificate, conductivity guarantee, approval or grade equivalence is automatic; quotation controls remain disabled.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Cast / lot traceability to the producing mill
- Chemical analysis, including oxygen where specified
- Electrical conductivity and mechanical test results for the supplied temper, where ordered
- Supplier safety data sheet for beryllium-containing material
Material enquiry
Request a material quotation
C17200 Beryllium Copper (Alloy 25) supplied to your material form, dimensions and specification.