Representative nickel-aluminium bronze round bars

Materials Supply / Copper & Copper-Base Alloys

C63200 Nickel-Aluminium Bronze

UNS C63200 | ASTM B150 / B171 | naval NAB

C63200 has narrower aluminium, a required 1.2–2.0% manganese and iron not exceeding nickel. It is supplied in a light-annealed condition for seawater service.

It is not interchangeable with C63000, and no exact EN/BS equivalent was verified.

Imagery is illustrative metal product forms, not certified C63200 stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

CDA lists ASTM B150, B124, B171 and B283. Confirm forms, sizes and availability at enquiry.

  • Rod and bar
  • Forgings
  • Plate

Material overview

C63200 Nickel-Aluminium Bronze

A wrought nickel-aluminium bronze with controlled aluminium, iron and manganese, used for seawater shafts, fasteners and valve parts.

  • All CDA typicals are in O50 light-anneal temper; no O20 or TQ50 data are shown.
  • Def Stan 02-833 covers wrought NAB but does not establish C63200 equivalence; 02-747 covers castings.

Designations and specifications

Designations and specifications
Designation / standardScope and qualification
UNSC63200
EN / BSNo exact equivalent verified
ASTM B150 / B124 / B171 / B283Rod/bar/shapes; forging stock; plate; die forgings
MIL-E-23765/3Welding electrodes, not structural stock
QQ-C-465Cited by Aviva; status not verified
Def Stan 02-833 Part 2Wrought NAB forgings, rods and sections — equivalence to C63200 not established
Not this gradeAMS4640 (C63000); Def Stan 02-747 (castings)

Specification review

Technical verification requirements

  • Heat treatment

    675°C specification temper anneal unverified.

    Obtain the governing specification.

  • Specifications

    Def Stan 02-833 and QQ-C-465 applicability unverified; specification minima not shown.

    Obtain controlled standards.

Grade selection

C63000 and C63200 — distinct wrought nickel-aluminium bronzes

C63000 and C63200 — distinct wrought nickel-aluminium bronzes
AspectC63000C63200Conventional aluminium bronze (context)
Aluminium (CDA)9.0–11.0%8.7–9.5%e.g. wrought C61400, cast C95400
Nickel incl. Co (CDA)4.0–5.5%4.0–4.8%No deliberate nickel addition
Iron / manganese (CDA)Fe 2.0–4.0%; Mn ≤1.5%Fe 3.5–4.3% (≤ Ni); Mn 1.2–2.0%—
CDA typical conditionM30 hot extruded; HR50 drawn + stress relievedO50 light anneal—
AMSAMS4640 (HR50 / TQ50)AMS4640 not established—
Typical roleAerospace bearings, bushings, gearsSeawater fasteners, shafts, valve stems—

C63000 and C63200 are not interchangeable. Conventional aluminium bronzes and cast nickel-aluminium bronzes (C95500, C95800) have separate chemistry and qualification; their properties are not transferable to these wrought grades.

Copper Development Association — C63200 alloy record

Engineering reference

Technical data

Chemical composition — CDA limits
ElementMass %
Aluminium8.7–9.5
Nickel (incl. Co)4.0–4.8
Iron3.5–4.3 (must not exceed Ni)
Manganese1.2–2.0
Silicon0.10 max
Lead0.02 max
Copper (incl. Ag)Remainder
Cu + named elements99.5 min

Elements not listed are not implied to be zero.

Copper Development Association — C63200 alloy record

Physical properties — C63200
PropertyValueBasis
Density7.64 g/cm³ (0.276 lb/in³)20°C
Electrical conductivity7% IACS20°C; temper not stated
Thermal conductivity34.6 W/(m·K) (20 Btu/h·ft·°F)20°C
Mean CTE 20–300°C16.2 × 10⁻⁶/KTemper not stated
Elastic modulus (tension)117 GPa (17,000 ksi)Temperature not stated
Modulus of rigidity44 GPa (6,400 ksi)Temperature not stated

CDA alloy-level values; temper, form and section not stated.

Copper Development Association — C63200 alloy record

Forging — O50 light anneal

C63200 — Forging — O50 light anneal
SectionTensile strengthYield (0.5% extension)ElongationHardness
5 in (127 mm)100 ksi (690 MPa)45 ksi (310 MPa)22%HRB 92

CDA typical values at 20°C, not specification minima.

Copper Development Association — C63200 alloy record

Plate — O50 light anneal

C63200 — Plate — O50 light anneal
SectionTensile strengthYield (0.5% extension)ElongationHardness
0.25 in (6.4 mm)100 ksi (690 MPa)50 ksi (345 MPa)20%HRB 92
0.5 in (12.7 mm)95 ksi (655 MPa)47 ksi (324 MPa)22%HRB 89
1 in (25 mm)90 ksi (621 MPa)45 ksi (310 MPa)25%HRB 85

CDA typical values at 20°C, not specification minima.

Copper Development Association — C63200 alloy record

Rod — O50 light anneal

C63200 — Rod — O50 light anneal
SectionTensile strengthYield (0.5% extension)ElongationHardness
1 in (25 mm)105 ksi (724 MPa)53 ksi (365 MPa)22%HRB 96
2 in (51 mm)103 ksi (710 MPa)52 ksi (359 MPa)24%HRB 94
3 in (76 mm)102 ksi (703 MPa)51 ksi (352 MPa)24%HRB 93

CDA typical values at 20°C, not specification minima.

Copper Development Association — C63200 alloy record

Annealing range (CDA)

621–704°C (1150–1300°F); soak and cooling not stated.

Specification temper anneal

A commonly quoted 675°C temper anneal lies within the CDA range but was not verified as a specification setpoint, tolerance or duration.

Not a complete production schedule; follow the ordered specification.

Copper Development Association — C63200 alloy record

Typical applications

Engineering applications

  • Seawater fasteners and shafts
  • Valve stems, seawater valves and pump bodies
  • Bearings and bushes

Subsequent manufacturing

Machining & processing

Wrought, not cast

These are wrought grades; cast nickel-aluminium bronze properties and specifications (e.g. Def Stan 02-747 castings) do not apply.

Machining and welding

Machinability and weld procedures must be qualified for the grade; C63200 welding electrodes fall under a separate specification.

Application evidence

Listed applications are source-cited categories, not claims of stock or component approval.

Material certification & testing

Documentation must be agreed for the actual UNS/EN grade, product or casting specification, form, temper and section.

No certificate, approval or grade equivalence is automatic. “Nearest” or “related” designations do not certify compliance; quotation controls remain disabled.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Cast / lot traceability to the producing mill or foundry
  • Chemical analysis and mechanical test results to the ordered specification
  • Ultrasonic, impact or corrosion-related testing only where the ordered specification requires it

Material enquiry

Request a material quotation

C63200 Nickel-Aluminium Bronze supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.