Representative turned high-strength steel round bars

Materials Supply / Maraging Steels

Maraging 300 (18Ni 300)

18Ni 300 | UNS K93120 | AMS6514

Maraging 300 has higher cobalt and titanium than Maraging 250, giving higher aged strength with lower ductility. It is supplied solution annealed and aged after machining.

It is not a precipitation-hardening stainless steel and is not interchangeable with Maraging 250 or 350.

Imagery is illustrative steel product forms, not certified Maraging 300 stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

AMS6514 covers bars, forgings, tubing and rings; BÖHLER lists V300 long products and plate. The 300-grade sheet specification AMS6521C was cancelled in 2005. Confirm forms, sizes and availability at enquiry.

  • Round bar and long products
  • Forgings and rings
  • Mechanical tubing
  • Plate

Material overview

Maraging 300 (18Ni 300)

An 18% nickel, 9% cobalt maraging steel aged to around 2 GPa tensile strength, widely used for ultra-high-strength components.

  • Solution-annealed and aged properties are shown as separate conditions.
  • VascoMax recommends ageing at 482–496°C (900–925°F) for 6 h to 50–55 HRC; Aubert & Duval MY19 recommends 480°C for 3–5 h.

Designations and product specifications

Designations and product specifications
Designation / standardScope and qualification
UNSK93120 (Aubert & Duval)
EuropeanX2NiCoMo18-9-5; producer documents give both 1.6358 and 1.6354 — unresolved
Producer namesVascoMax C-300; MY19; BÖHLER V300 (VIM + VAR)
AMS6514Bars, forgings, tubing and rings; consumable-electrode vacuum melted, annealed — current revision not authenticated
AMS6521CSheet, strip and plate — cancelled 22 September 2005
ASTM A579/A579M-20Superstrength alloy-steel forgings — withdrawn 2024

Consumable-electrode vacuum melting alone does not establish VIM + VAR; specify the melt route. Obtain controlled current standards before ordering.

SAE AMS6514 — official catalogue entry (current revision not authenticated)

Specification review

Technical verification requirements

  • Specifications

    Current AMS6514 revision and acceptance limits not authenticated; no current 300-grade sheet AMS verified.

    Obtain controlled current AMS texts.

  • Designations

    European number 1.6358 vs 1.6354 conflicts between producer documents.

    Confirm the European number with the producer.

  • Mechanical evidence

    VascoMax aged table omits the ageing cycle; MY19 KV temperature conflict.

    Obtain mill test data with full treatment and test basis.

Grade selection

Maraging 250, 300 and 350 — distinct grades

Maraging 250, 300 and 350 — distinct grades
AspectMaraging 250Maraging 300Maraging 350
Cobalt (VascoMax nominal)7.50%9.00%12.00%
Titanium (VascoMax nominal)0.40%0.60%1.40%
Nickel / molybdenum (nominal)18.50% / 4.80%18.50% / 4.80%18.50% / 4.80%
UNSK92890K93120Not verified
Bar / forging AMSAMS6512AMS6514AMS6515 (double vacuum melted)
Sheet / strip / plate AMSAMS6520AMS6521C — cancelled 2005None verified
Aged ⅝-in round, longitudinal (typical)264.5 ksi UTS; 11.5% El.294.0 ksi UTS; 11.8% El.350.2 ksi UTS; 7.5% El.

18Ni maraging steels are low-carbon iron–nickel–cobalt–molybdenum steels hardened by intermetallic precipitation on ageing; they are not precipitation-hardening stainless steels such as 17-4PH. Aged values are VascoMax nominal results; the table does not state their ageing cycle. Higher strength comes with lower ductility; substitution requires engineering approval.

Engineering reference

Technical data

Chemical composition — VascoMax C-300 nominal analysis
ElementNominal mass %
Nickel18.50
Cobalt9.00
Molybdenum4.80
Titanium0.60
Aluminium0.10
Carbon0.03 max
Silicon0.10 max
Manganese0.10 max
Sulphur0.01 max
Phosphorus0.01 max
Zirconium0.01
Boron0.003
IronBalance

Producer nominal analysis, not specification limits. Aubert & Duval MY19 reports C ≤0.010, Ni 18.00, Co 8.75, Mo 4.90, Ti 0.70, Al 0.10.

Physical properties — Aubert & Duval MY19 and VascoMax C-300
PropertyProducer valueBasis
Density8.0 g/cm³ (0.289 lb/in³)VascoMax; condition not stated
Elastic modulus195 GPaMY19, 20°C
Torsional modulus72 GPaMY19
Thermal conductivity20.5 W/(m·K)MY19, 20°C
Thermal conductivity21.8 W/(m·K)MY19, 100°C
Mean CTE — solution treated9.9 × 10⁻⁶ /KMY19, 0–100°C
Mean CTE — aged9.5 × 10⁻⁶ /KMY19, 0–100°C
Mean CTE — aged10.6 × 10⁻⁶ /KMY19, 0–300°C

VascoMax gives a modulus of 27.5 × 10⁶ psi (190 GPa) and conductivity 14.6 Btu/ft·h·°F at 68°F; values are kept with their own sources rather than merged.

Solution annealed — VascoMax nominal

Maraging 300 — nominal annealed properties
PropertyProducer nominalBasis
Ultimate tensile strength1034 MPa (150 ksi)Nominal
Yield strength758 MPa (110 ksi)Offset not stated
Elongation18%Gauge not stated
Reduction of area72%Nominal
Hardness32 HRCNominal

VascoMax “Nominal Annealed Properties”. Section, orientation, gauge length and test temperature not stated. Typical values, not specification limits.

Aged — ⅝-in round bar, longitudinal — VascoMax nominal

Maraging 300 — aged, ⅝-in round bar (longitudinal)
PropertyProducer nominalBasis
Ultimate tensile strength2027 MPa (294.0 ksi)Room temperature
0.2% yield strength2000 MPa (290.0 ksi)Room temperature
Elongation11.8%4.5√A gauge
Reduction of area56.6%Room temperature
Hardness54.3 HRCRoom temperature

VascoMax “Nominal Room Temperature Properties after Aging”. The table does not state the ageing cycle, so none is attached. Nominal values for this form and orientation only; not specification minima or design allowables.

Aged — 0.250-in sheet, transverse — VascoMax nominal

Maraging 300 — aged, 0.250-in sheet (transverse)
PropertyProducer nominalBasis
Ultimate tensile strength2169 MPa (314.6 ksi)Room temperature
0.2% yield strength2135 MPa (309.7 ksi)Room temperature
Elongation7.7%4.5√A gauge
Reduction of area35.0%Room temperature
Hardness55.1 HRCRoom temperature

VascoMax “Nominal Room Temperature Properties after Aging”. The table does not state the ageing cycle, so none is attached. Nominal values for this form and orientation only; not specification minima or design allowables.

MY19 — solution 820°C + aged 480°C 4 h — typical

MY19 (Maraging 300 type) — typical properties
ConditionUTS0.2% YSElongation (5d)Other
Solution treated 820°C, air cooled1070 MPa870 MPa14%RA 70%; <36 HRC
Aged 480°C × 4 h, tested 20°C2050 MPa1980 MPa8.5%RA 53%; KIc 65 MPa√m; KV 25 J; 53 HRC

Aubert & Duval typical values; product form, section and orientation not stated. The KV test temperature conflicts between PDF (20°C) and webpage (−60°C). Typical, not guaranteed limits.

Solution annealing

802–829°C (1475–1525°F); minimum 1 h for 25 mm (1 in) thickness plus 1 h per additional 25 mm; air cool.

Ageing

482–496°C (900–925°F) for 6 h, air cool; 50–55 HRC.

Section size

Larger sections require longer ageing periods; qualify the cycle for the actual section.

VascoMax recommendations for Maraging 300. The schedules are producer guidance, not universal acceptance treatments; component cycles must be qualified.

Typical applications

Engineering applications

  • Ultra-high-strength aerospace structural parts
  • Missile and rocket-motor bodies
  • Centrifuge components
  • Die-casting tooling

Subsequent manufacturing

Machining & processing

Machining

Normally machined in the solution-annealed condition, then aged; ageing causes only small dimensional change, which should be confirmed for the part.

Not a stainless steel

Maraging steels are not corrosion-resistant stainless grades; surface protection must be specified for the service environment.

Welding

Welding requires a qualified procedure with post-weld ageing; weld properties are not implied by base-metal data.

Application evidence

Listed applications are producer-cited categories, not claims of stock or component approval.

Material certification & testing

Documentation and inspection must be agreed for the actual grade, specification revision, melting route, product form, section and delivery condition (normally solution annealed).

No certificate, test, aerospace approval or grade equivalence is automatic. Maraging grades 250, 300 and 350 are not interchangeable; quotation controls remain disabled.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the producing mill
  • Chemical analysis and mechanical test reports to the ordered specification
  • Ageing-response test results on supplied material, where required
  • Melting-route evidence (e.g. VIM + VAR), ultrasonic inspection or customer-specific testing only where agreed

Material enquiry

Request a material quotation

Maraging 300 (18Ni 300) supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.