Representative extruded aluminium alloy round bars

Materials Supply / Aluminium Alloys

Aluminium Alloy 2011

Free-machining aluminium-copper alloy | UNS A92011 | EN AW-2011 (AlCu6BiPb)

Aluminium alloy 2011 is a heat-treatable aluminium-copper alloy containing lead and bismuth, which break chips and lower cutting forces in automatic turning.

It is a turned-parts alloy, not a default choice for critical aerospace structural components.

Imagery is illustrative only; it does not identify a certified alloy, temper or available stock.

Raw & semi-finished materials

Available material forms

Kaiser supplies cold-finished rod and bar to ASTM B211; T6 is associated with extruded bar and tube in European sources. Supply remains subject to supplier, specification, temper and dimensional confirmation; no Quest stockholding is implied.

  • Round bar (cold finished)
  • Hexagon and flat bar
  • Extruded bar and tube (T6)

Material overview

Aluminium Alloy 2011

Free-machining aluminium-copper alloy with lead and bismuth additions, suited to high-volume precision turned components.

  • Kaiser rates 2011 machinability A — the highest rating in its scale — with short, broken chips and good surface finish in automatic lathe work.
  • The free-machining additions limit other properties: Kaiser rates corrosion resistance and anodising response only fair and does not recommend welding other than resistance welding.
  • Lead content raises regulatory questions (RoHS, ELV). Sources disagree on scope: Kaiser states its post-2009 rod is RoHS compliant, while Müller & Welte states its EN AW-2011 does not meet RoHS/ELV. Confirm the applicable exemption, market and certificate. EN AW-2011A also contains lead and is not a lead-free grade.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
UNSA92011
EN AWEN AW-2011 / AlCu6BiPb
ASTM B211Cold-finished rod and bar (Kaiser). Current revision not accessed.
AMS-QQ-A-225/3Rod and bar (Kaiser). Current revision not accessed.
EN 573-3 / EN 754European chemistry and drawn-bar standards — full texts not accessed

No SAE AMS aerospace specification was verified for 2011.

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

  • Lead / RoHS / ELV

    Producer bulletin reports a May 2009 Pb cap change to 0.4% and advises checking certification. This does not independently establish current market/exemption applicability for all registered 2011 (Pb up to 0.6%).

    Obtain current legal exemption basis, product category, date/market and batch analysis; retain explicit lead-bearing warning.

Grade selection

2011 compared with 2014

2011 compared with 2014
Aspect20112014
Registered chemistry (AA)Cu 5.0–6.0; Pb 0.20–0.6; Bi 0.20–0.6Cu 3.9–5.0; Si 0.50–1.2; Mn 0.40–1.2; Mg 0.20–0.8
Primary purposeFree-machining turned parts (Pb/Bi chip breakers)High-strength heat-treatable forgings and structural parts
MachinabilityRated A by Kaiser; short chipsGood machinability (supplier statement); not free-machining
Fabrication limitsWelding not recommended except resistance welding (fair); anodising only fair; lead regulationLower corrosion resistance — protective finishing advised
Typical applicationsScrew-machine and precision turned partsAircraft fittings, forgings, high-load machined parts

Qualitative comparison only. No numerical strength comparison is shown because no directly comparable temper and product-form data were verified for both alloys.

The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025

Engineering reference

Technical data

Chemical composition limits — 2011 (AA)
ElementMass %Limit
AlRemainderBalance
Cu5.0–6.0Range
Pb0.20–0.6Range
Bi0.20–0.6Range
Si0.40Maximum
Fe0.7Maximum
Zn0.30Maximum

Aluminum Association registered limits; single values are maximums. Al is the remainder (balance). Other elements: 0.05% each, 0.15% total maximum. Kaiser limits its own Pb to 0.20–0.40% (since May 2009); this is a producer restriction, not the registered limit. Confirm against the ordered specification and mill certificate.

The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025

Physical properties — producer typical
PropertyValueTemper / basis
Density2820 kg/m³Kaiser nominal at 20°C
Elastic modulus70 GPaKaiser
Melting range541–638°CKaiser
Specific heat864 J/kg·K100°C
Thermal expansion23.1 × 10⁻⁶ K⁻¹20–100°C
Thermal conductivity152 W/m·K (T3); 173 W/m·K (T8)20°C
Electrical conductivity39% IACS (T3); 45% IACS (T8)20°C; equal-volume basis

Kaiser typical values. Müller & Welte gives slightly different rounded values.

T3 rod and bar — producer typical

T3 rod and bar — producer typical
PropertyValue
Ultimate tensile strength379 MPa
Yield strength296 MPa
Elongation15%
Brinell hardness95
Shear strength221 MPa
Fatigue endurance limit (5×10⁸ cycles)124 MPa

Kaiser typical values, 12.7 mm (0.500 in) specimen, room temperature. Not specification minimums. Kaiser identifies elongation/4D (50.8 mm for the 12.7 mm tensile specimen); stock section and tensile orientation are not specified. The specimen diameter is not an offered-stock dimensional limit.

T8 rod and bar — producer typical

T8 rod and bar — producer typical
PropertyValue
Ultimate tensile strength407 MPa
Yield strength310 MPa
Elongation12%
Brinell hardness100
Shear strength241 MPa
Fatigue endurance limit (5×10⁸ cycles)124 MPa

Kaiser typical values, 12.7 mm specimen, room temperature. Not specification minimums; not interchangeable with T3. Kaiser identifies elongation/4D (50.8 mm for the 12.7 mm tensile specimen); stock section and tensile orientation are not specified. The specimen diameter is not an offered-stock dimensional limit.

Temper designations (ANSI H35.1 summary)

T3: solution heat treated, cold worked, naturally aged. T4: solution heat treated, naturally aged. T6: solution heat treated, artificially aged. T8: solution heat treated, cold worked, artificially aged. A following 51 (e.g. T351, T651, T851) means stress relieved by controlled stretching; 510/511 apply to extruded products (511 allows minor straightening); 52 means stress relieved by compression. Not every alloy is produced in every temper or form.

Heat-treatment limitations

No producer solution or ageing temperatures were verified. Lead and bismuth have low melting points, so overheating risks incipient melting; follow the ordered specification.

Schedules are not copied from other 2000-series alloys. No verified T6 property table is shown.

ANSI H35.1 temper designation system (The Aluminum Association) — summary; full standard not accessed

Material selection

Corrosion resistance & performance

Kaiser rates general corrosion resistance only fair; Müller & Welte describes moderate atmospheric and poor seawater resistance. Protective finishing is normally needed.

Anodising response is only fair; decorative and hard anodising are described as less suitable.

Free-machining additions can reduce corrosion performance; performance depends on temper and environment.

Typical applications

Engineering applications

  • Precision turned components
  • Automatic lathe and screw-machine parts
  • Fittings
  • Screws, bolts, nuts and threaded components
  • Instrument components
  • General precision engineering

Subsequent manufacturing

Machining & processing

Machining

Excellent machinability with short chips, low cutting forces and good surface finish; suited to automatic lathes. Machining parameters depend on temper, tooling, set-up and part geometry; no universal cutting speed is given. Machining of stress-relieved (…51) tempers reduces, but does not eliminate, distortion from residual stress.

Welding

Kaiser rates weldability poor and does not recommend welding methods other than resistance welding (fair).

Regulatory

Lead-bearing. Confirm RoHS/ELV status with the supplier certificate; see the ELV exemption guidance from European Aluminium.

Material certification & testing

Agree documentation and inspection at enquiry stage. Alloy designation alone does not define compliant aerospace material — the specification, temper, product form and dimensions must also be confirmed.

Not every test or certificate is automatically included. These records do not confer aerospace approval.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch (cast) traceability to the mill certificate
  • Chemical analysis and temper verification
  • Mechanical testing and hardness testing to the ordered specification
  • Heat-treatment records
  • Ultrasonic, aerospace-specific or customer-specific inspection only where applicable and agreed

Material enquiry

Request a material quotation

Aluminium Alloy 2011 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.