Materials Supply / Aluminium Alloys
Aluminium Alloy 2124
Controlled-impurity aerospace plate alloy | UNS A92124 | EN AW-2124 | T851
Aluminium alloy 2124 has the same copper, magnesium and manganese ranges as 2024 but lower iron (0.30% max) and silicon (0.20% max) limits.
Alcoa states the plate was developed with guaranteed fracture toughness and improved short-transverse properties in thick sections. It is not universally stronger than 2024.
Imagery is illustrative only; it does not identify a certified alloy, temper or available stock.
Raw & semi-finished materials
Available material forms
Kaiser states T851 plate is commonly supplied 38–152 mm (1.5–6.0 in) thick; Alcoa gives the same range. Supply remains subject to supplier, specification, temper and dimensional confirmation; no Quest stockholding is implied.
- Plate
- Cut-to-size plate
Material overview
Aluminium Alloy 2124
High-purity version of 2024 with tighter iron and silicon limits, supplied as thick T851 plate for damage-tolerant aircraft structures.
- Lower iron and silicon reduce coarse intermetallic particles, which is the metallurgical basis for better fracture toughness in thick plate.
- Only T851 plate is shown. Minimum properties fall with thickness, and toughness depends strongly on orientation.
- Alcoa describes strength retention and creep resistance to 177°C and recommends 121–177°C applications; this is a producer application statement, not a maximum service temperature.
Designations and product specifications
| Designation / standard | Scope / status |
|---|---|
| UNS | A92124 |
| EN AW | EN AW-2124 / AlCu4Mg1(A) — confirm against EN 573-3 |
| AMS 4101 | T851 plate, 25–152 mm (thyssenkrupp listing) |
| AMS-QQ-A-250/29, ASTM B209 | Plate (thyssenkrupp listing) |
Current AMS and EN 485 texts not accessed. AMS 4221 is quoted by one supplier without a stated temper or form and is not shown.
Specification review
Technical verification requirements
Designations / form / temper / dimensions
Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.
Obtain applicable controlled specification and producer confirmation; submit to technical review.
Mechanical conditions / gauge / orientation
Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.
Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.
Fracture toughness research citation
Specific 30/40/55 mm research means need exact study citation, test validity and orientation evidence. They are appropriately called research, not guaranteed minima.
Obtain applicable controlled specification and producer confirmation; submit to technical review.
Grade selection
2024 compared with 2124
| Aspect | 2024 | 2124 |
|---|---|---|
| Si, maximum | 0.50% | 0.20% |
| Fe, maximum | 0.50% | 0.30% |
| Cu / Mg / Mn | 3.8–4.9 / 1.2–1.8 / 0.30–0.9 | 3.8–4.9 / 1.2–1.8 / 0.30–0.9 (same) |
| Main product forms (sources) | Bare and Alclad sheet, plate, bar, tube | Thick plate, T851 (Kaiser: commonly 38–152 mm) |
| Distinguishing aim | General high-strength aircraft alloy; fatigue performance | Controlled impurities for thick-plate fracture toughness and short-transverse properties (Alcoa) |
| Typical applications | Aircraft structural sheet, plate, fittings | Machined bulkheads and wing structures (Alcoa) |
Composition from Aluminum Association Teal Sheets. 2124 is not universally stronger than 2024; no like-for-like strength comparison on the same specification, thickness and orientation was found, so none is shown.
The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025
Engineering reference
Technical data
| Element | Mass % | Limit |
|---|---|---|
| Al | Remainder | Balance |
| Cu | 3.8–4.9 | Range |
| Mg | 1.2–1.8 | Range |
| Mn | 0.30–0.9 | Range |
| Si | 0.20 | Maximum |
| Fe | 0.30 | Maximum |
| Cr | 0.10 | Maximum |
| Zn | 0.25 | Maximum |
| Ti | 0.15 | Maximum |
Aluminum Association registered limits; single values are maximums. Al is the remainder (balance). Other elements: 0.05% each, 0.15% total maximum. Footnote 7: a Zr+Ti limit of 0.20% maximum may be used for extruded and forged products only, by producer–purchaser agreement. Confirm against the ordered specification and mill certificate.
The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025
| Property | Value | Temper / basis |
|---|---|---|
| Density | 2770 kg/m³ | Kaiser nominal |
| Elastic modulus | 73.1 GPa | Kaiser |
| Melting range | 502–638°C | Kaiser |
| Specific heat | 875 J/kg·K | 100°C |
| Thermal expansion | 22.9 × 10⁻⁶ K⁻¹ | 20–100°C |
| Thermal conductivity | 151 W/m·K | T851, 20°C |
| Electrical conductivity | 39% IACS | T851, 20°C |
Kaiser typical values.
T851 plate — producer typical
| Property | Value |
|---|---|
| Ultimate tensile strength | 485 MPa |
| Yield strength | 450 MPa |
| Elongation | 8% |
Kaiser typical values, 12.7 mm round specimen; not thickness-specific minimums.
T851 plate 25–50 mm — supplier table
| Property | Value |
|---|---|
| Ultimate tensile strength | 455 MPa |
| Yield strength | 393 MPa |
| Elongation | 5% |
Smiths Metal Centres table for 25.4–50.8 mm (1.001–2.00 in); statistical basis and orientation not stated.
T851 plate 127–152 mm — supplier table
| Property | Value |
|---|---|
| Ultimate tensile strength | 434 MPa |
| Yield strength | 372 MPa |
| Elongation | 4% |
Smiths Metal Centres table for 127–152 mm (5.001–6.00 in); statistical basis and orientation not stated.
Temper designations (ANSI H35.1 summary)
T3: solution heat treated, cold worked, naturally aged. T4: solution heat treated, naturally aged. T6: solution heat treated, artificially aged. T8: solution heat treated, cold worked, artificially aged. A following 51 (e.g. T351, T651, T851) means stress relieved by controlled stretching; 510/511 apply to extruded products (511 allows minor straightening); 52 means stress relieved by compression. Not every alloy is produced in every temper or form.
T851
Solution heat treated, stress relieved by controlled stretching, then artificially aged. No producer-verified temperatures were found; use the ordered specification.
The 2024 temper list is not copied to 2124; only T851 plate is verified.
ANSI H35.1 temper designation system (The Aluminum Association) — summary; full standard not accessed
Material selection
Corrosion resistance & performance
Kaiser rates T851 general corrosion D and stress corrosion B; general corrosion resistance and anodisability are only fair.
Smiths states poor atmospheric corrosion resistance but excellent exfoliation resistance. Protective finishing is required.
Typical applications
Engineering applications
- Aerospace plate
- Machined fuselage bulkheads (Alcoa)
- Wing structures (Alcoa)
- Damage-tolerant aerospace components, where specified and approved
- High-integrity machined parts
Subsequent manufacturing
Machining & processing
Machining
Kaiser rates machinability B. Thick T851 plate is used for high-integrity machined parts; stretch stress relief limits distortion. Machining parameters depend on temper, tooling, set-up and part geometry; no universal cutting speed is given. Machining of stress-relieved (…51) tempers reduces, but does not eliminate, distortion from residual stress.
Fracture toughness
One study of 2124-T851 plate (30, 40 and 55 mm) measured mean K1c of 28.9–33.0 MPa√m in L-T and 23.9–24.9 MPa√m in T-L. These are research results, not guaranteed minimums.
Welding
Kaiser rates gas welding D, arc C and spot B.
Material certification & testing
Agree documentation and inspection at enquiry stage. Alloy designation alone does not define compliant aerospace material — the specification, temper, product form and dimensions must also be confirmed.
Not every test or certificate is automatically included. These records do not confer aerospace approval.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Heat / batch (cast) traceability to the mill certificate
- Chemical analysis and temper verification
- Mechanical testing and hardness testing to the ordered specification
- Heat-treatment records
- Ultrasonic, aerospace-specific or customer-specific inspection only where applicable and agreed
Material enquiry
Request a material quotation
Aluminium Alloy 2124 supplied to your material form, dimensions and specification.