Representative aluminium alloy plates with sawn edges

Materials Supply / Aluminium Alloys

Aluminium Alloy 2219

Weldable aluminium-copper alloy for elevated and cryogenic temperatures | UNS A92219 | EN AW-2219 (AlCu6Mn)

Aluminium alloy 2219 is a heat-treatable aluminium-copper-manganese alloy with vanadium and zirconium additions.

Kaiser rates it A for gas, arc and spot welding and describes it as useful from −269°C to 316°C (−452°F to 600°F). This is a descriptive range, not a maximum continuous service temperature.

Imagery is illustrative only; it does not identify a certified alloy, temper or available stock.

Raw & semi-finished materials

Available material forms

Forms linked to 2219 in the Aircraft Materials specification index; tempers differ by form. Supply remains subject to supplier, specification, temper and dimensional confirmation; no Quest stockholding is implied.

  • Sheet and plate (bare and Alclad)
  • Extrusions
  • Forgings and rings
  • Seamless tube

Material overview

Aluminium Alloy 2219

Weldable high-copper aluminium alloy used for welded space-booster tanks and elevated-temperature aerospace structures.

  • Separate conditions are shown for T351, T37, T851 and T87 sheet/plate and for T8511 extrusions. All values are typical.
  • No numerical elevated-temperature or cryogenic tensile table with exposure duration was verified, so no High-Temperature Performance table is shown. T31, T62 and T81 property data were not verified.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
UNSA92219
EN AWEN AW-2219 / AlCu6Mn
AMS 4031O / F sheet and plate
AMS 4094T81 Alclad sheet / T851 Alclad plate
AMS 4095T31 Alclad sheet / T351 Alclad plate
AMS 4143T6 forgings and rolled or forged rings
AMS 4144T852 / T851 hand forgings
AMS 4162T8511 extrusions
AMS 4066 / AMS 4068T8511 / T3511 drawn seamless tubing

From the Aircraft Materials specification index; current revisions and scopes not accessed.

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

Grade selection

2219 compared with 2618 / 2618A

2219 compared with 2618 / 2618A
Aspect22192618 / 2618A
Alloy systemAl-Cu-Mn with V and Zr (Cu 5.8–6.8)Al-Cu-Mg-Fe-Ni (Cu ~1.8–2.7, Fe and Ni ~0.8–1.4)
Heat-treatment responseSolution treated; naturally or artificially aged, with or without cold work (T3x, T6x, T8x)Solution treated and artificially aged (T6, T6511 per sources)
Elevated temperature (producer statements)Useful from −269°C to 316°C (Kaiser / Aircraft Materials)Strength retained relatively well to ~200°C; used up to 300°C (Smiths / Leichtmetall)
Weldability (producer ratings)Rated A for gas, arc and spot welding (Kaiser T351/T851)Conflicting producer statements — confirm per product
Typical applicationsWelded space-booster and fuel tanks, elevated-temperature structuresAerospace and high-temperature mechanical components

Qualitative producer comparison. No numerical elevated-temperature tensile data with exposure duration were verified for either alloy, so no strength comparison or maximum service temperature is given.

The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025

Engineering reference

Technical data

Chemical composition limits — 2219 (AA)
ElementMass %Limit
AlRemainderBalance
Cu5.8–6.8Range
Mn0.20–0.40Range
Zr0.10–0.25Range
V0.05–0.15Range
Ti0.02–0.10Range
Si0.20Maximum
Fe0.30Maximum
Mg0.02Maximum
Zn0.10Maximum

Aluminum Association registered limits; single values are maximums. Al is the remainder (balance). Other elements: 0.05% each, 0.15% total maximum. Confirm against the ordered specification and mill certificate.

The Aluminum Association — International Alloy Designations and Chemical Composition Limits (Teal Sheets), August 2025

Physical properties
PropertyValueBasis
Density2840 kg/m³AA nominal
Elastic modulus73.1 GPaKaiser, listed tempers

Other physical properties were not verified on a temper-identified basis and are omitted.

T351 sheet and plate — producer typical

T351 sheet and plate — producer typical
PropertyValue
Ultimate tensile strength359 MPa
Yield strength248 MPa
Elongation17%

Kaiser typical, longitudinal, 12.7 mm round specimen.

T37 sheet and plate — producer typical

T37 sheet and plate — producer typical
PropertyValue
Ultimate tensile strength393 MPa
Yield strength317 MPa
Elongation11%

Kaiser typical, longitudinal.

T851 sheet and plate — producer typical

T851 sheet and plate — producer typical
PropertyValue
Ultimate tensile strength455 MPa
Yield strength352 MPa
Elongation10%
Fatigue endurance limit (5×10⁸ cycles, R.R. Moore)103 MPa

Kaiser typical, longitudinal.

T87 sheet and plate — producer typical

T87 sheet and plate — producer typical
PropertyValue
Ultimate tensile strength476 MPa
Yield strength393 MPa
Elongation10%

Kaiser typical, longitudinal.

T8511 extrusions — typical

T8511 extrusions — typical
PropertyValue
Ultimate tensile strength (L / LT)400 / 386 MPa
Yield strength (L / LT)290 / 269 MPa
Elongation (L / LT)6% / 4%

Aircraft Materials typical values (AMS 4162 listed).

Temper designations (ANSI H35.1 summary)

T3: solution heat treated, cold worked, naturally aged. T4: solution heat treated, naturally aged. T6: solution heat treated, artificially aged. T8: solution heat treated, cold worked, artificially aged. A following 51 (e.g. T351, T651, T851) means stress relieved by controlled stretching; 510/511 apply to extruded products (511 allows minor straightening); 52 means stress relieved by compression. Not every alloy is produced in every temper or form.

T37 and T87

Solution heat treated and cold worked by a larger specified amount before natural (T37) or artificial (T87) ageing. No producer-verified temperatures were found.

Schedules are not copied from other alloys. Kaiser reports good stress-corrosion cracking resistance in T8 tempers.

ANSI H35.1 temper designation system (The Aluminum Association) — summary; full standard not accessed

Material selection

Corrosion resistance & performance

Kaiser rates T351/T851 general corrosion D; stress corrosion C (T351) and B (T851). Protective finishing is required.

Alclad sheet and plate (AMS 4094–4096) carry protective cladding.

Typical applications

Engineering applications

  • Welded aerospace assemblies
  • Space-booster propellant and fuel tanks
  • Spacecraft components, where specified and approved
  • Elevated-temperature structural applications

Subsequent manufacturing

Machining & processing

Welding

Rated A for gas, arc and spot welding (Kaiser, T351/T851). Qualify the procedure and filler for the ordered temper.

Machining

Machining parameters depend on temper, tooling, set-up and part geometry; no universal cutting speed is given. Machining of stress-relieved (…51) tempers reduces, but does not eliminate, distortion from residual stress.

Temperature range

Producer descriptions cite use from −269°C to 316°C with good fracture toughness; no numerical tensile-versus-temperature data were verified.

Material certification & testing

Agree documentation and inspection at enquiry stage. Alloy designation alone does not define compliant aerospace material — the specification, temper, product form and dimensions must also be confirmed.

Not every test or certificate is automatically included. These records do not confer aerospace approval.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch (cast) traceability to the mill certificate
  • Chemical analysis and temper verification
  • Mechanical testing and hardness testing to the ordered specification
  • Heat-treatment records
  • Ultrasonic, aerospace-specific or customer-specific inspection only where applicable and agreed

Material enquiry

Request a material quotation

Aluminium Alloy 2219 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.