Materials Supply / Copper & Copper-Base Alloys
C52100 Phosphor Bronze (8% Sn)
UNS C52100 | ASTM B103 / B139 / B159 | approx. CW453K
C52100 has higher tin than C51000, giving higher strength at each temper with lower conductivity. Its nearest European grade is CW453K (CuSn8, old BS PB104).
Properties are not transferred from C51000 or PB1.
Imagery is illustrative metal product forms, not certified C52100 stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
ASTM B103 flat products, B139 rod/bar/shapes, B159 wire. Confirm forms, sizes and availability at enquiry.
- Strip, sheet and plate
- Rod and bar
- Wire
Material overview
C52100 Phosphor Bronze (8% Sn)
A wrought 8% tin phosphor bronze, stronger than C51000, for springs, wear plates and high-stress contacts.
- CDA lists no O60 typical; the OS035 grain-size anneal (58 ksi, 65%) is a separate temper and is not relabelled.
- CW453K: Sn 7.5–8.5% (CDA UK) versus C52100 Sn 7.0–9.0%.
Designations and specifications
| Designation / standard | Scope and qualification |
|---|---|
| UNS | C52100 |
| EN / BS | Approximately CW453K CuSn8 / PB104 — chemistry limits differ |
| ASTM B103 / B139 / B159 | Flat products / rod, bar and shapes / wire |
| EN 1652 / EN 12163 | Flat products / rod for CW453K |
Specification review
Technical verification requirements
Mechanical
No O60 typical; wire yield and elongation unreported.
Obtain producer or specification data.
Grade selection
Phosphor and silicon bronzes — distinct grades
| Grade | Type | Key chemistry (limits) | Conductivity (CDA, 20°C) | Nearest EN / BS |
|---|---|---|---|---|
| C51000 | Wrought phosphor bronze | Sn 4.2–5.8%; P 0.03–0.35% | 15% IACS (5% Sn, 0.2% P basis) | Approx. CW451K CuSn5 / PB102 |
| C52100 | Wrought phosphor bronze | Sn 7.0–9.0%; P 0.03–0.35% | 13% IACS | Approx. CW453K CuSn8 / PB104 |
| PB1 | Cast phosphor bronze | Sn 10.0–11.5%; P 0.5–1.0% (EN 1982 CC481K casting) | Not stated as % IACS | Cross-referenced to CC481K CuSn11P-C |
| C65100 | Wrought low-silicon bronze | Si 0.8–2.0% | 12% IACS | Not CW116C |
| C65500 | Wrought high-silicon bronze | Si 2.8–3.8%; Mn 0.50–1.3% | 7% IACS | Related to CW116C CuSi3Mn1 / CS101 |
PB1 is a cast alloy and is not CW451K. UNS and EN chemistries differ, so “approximately” equivalent grades are not automatically cross-certified. Properties are never transferred between these grades.
Engineering reference
Technical data
| Element | Mass % |
|---|---|
| Tin | 7.0–9.0 |
| Phosphorus | 0.03–0.35 |
| Lead | 0.05 max |
| Zinc | 0.20 max |
| Iron | 0.10 max |
| Copper | Remainder |
| Cu + named elements | 99.5 min |
Copper Development Association — C52100 alloy record
| Property | Value | Basis |
|---|---|---|
| Density | 8.8 g/cm³ | From CDA specific gravity |
| Electrical conductivity | 13% IACS | 20°C |
| Thermal conductivity | 62.3 W/(m·K) | 20°C |
| Mean CTE 20–300°C | 18.2 × 10⁻⁶/K | Temper not stated |
| Elastic modulus (tension) | 110 GPa | Temperature not stated |
CDA generic values; temper, form and section not stated.
Copper Development Association — C52100 alloy record
Flat — H02 half hard
| Section | Tensile strength | Yield (0.2% offset) | Elongation | Hardness |
|---|---|---|---|---|
| 0.04 in (1.0 mm) | 77 ksi (531 MPa) | 64 ksi (441 MPa) | 34% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C52100 alloy record
Flat — H04 hard
| Section | Tensile strength | Yield (0.2% offset) | Elongation | Hardness |
|---|---|---|---|---|
| 0.04 in (1.0 mm) | 93 ksi (641 MPa) | 87 ksi (600 MPa) | 19% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C52100 alloy record
Flat — H08 spring
| Section | Tensile strength | Yield (0.2% offset) | Elongation | Hardness |
|---|---|---|---|---|
| 0.04 in (1.0 mm) | 112 ksi (772 MPa) | 108 ksi (745 MPa) | 5% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C52100 alloy record
Wire — H02 / H04 (tensile only)
| Section | Tensile strength | Yield (0.2% offset) | Elongation | Hardness |
|---|---|---|---|---|
| H02, 0.08 in (2.0 mm) | 105 ksi (724 MPa) | Not reported | Not reported | Not reported |
| H04, 0.08 in | 130 ksi (896 MPa) | Not reported | Not reported | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C52100 alloy record
Annealing range (CDA)
482–677°C (900–1250°F). Section, hold time and atmosphere are not stated; not a complete production schedule.
Temper designations
O60 soft anneal; H02 half hard; H04 hard; H08 spring. Grain-size anneals (OS) and O61 are separate tempers and are not relabelled.
Agree temper with the product specification.
Copper Development Association — C52100 alloy record
Typical applications
Engineering applications
- Heavy-duty springs and contacts
- Bearing and wear plates
- Bellows
Subsequent manufacturing
Machining & processing
Cold working
Good cold workability (CDA); hot forming poor.
Not heat-treatable
Strength comes from cold work (H tempers); annealing softens. Temper must be specified with the product form.
Application evidence
Listed applications are source-cited categories, not claims of stock or component approval.
Material certification & testing
Documentation must be agreed for the actual UNS/EN grade, product or casting specification, form, temper and section.
No certificate, approval or grade equivalence is automatic. “Nearest” or “related” designations do not certify compliance; quotation controls remain disabled.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Cast / lot traceability to the producing mill or foundry
- Chemical analysis and mechanical test results to the ordered specification
- Ultrasonic, impact or corrosion-related testing only where the ordered specification requires it
Material enquiry
Request a material quotation
C52100 Phosphor Bronze (8% Sn) supplied to your material form, dimensions and specification.