Materials Supply / Copper & Copper-Base Alloys
C65100 Low-Silicon Bronze
UNS C65100 | ASTM B96 / B98 / B99 / B315
C65100 has about half the silicon of C65500, with higher conductivity and lower strength. It is not CW116C.
Properties are not transferred from C65500.
Imagery is illustrative metal product forms, not certified C65100 stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
ASTM B96 flat, B98 rod/bar, B99 wire, B315 tube. Confirm forms, sizes and availability at enquiry.
- Strip, sheet and plate
- Rod and bar
- Wire
- Seamless pipe and tube
Material overview
C65100 Low-Silicon Bronze
A wrought low-silicon bronze (0.8–2.0% Si) for fasteners, marine and electrical hardware.
- Silicon-bronze yield is 0.5% extension, not 0.2% offset.
- No European equivalent verified.
Designations and specifications
| Designation / standard | Scope and qualification |
|---|---|
| UNS | C65100 |
| EN / BS | No equivalent verified; not CW116C |
| ASTM B96 / B98 / B99 / B315 | Flat / rod, bar, shapes / wire / seamless pipe and tube |
Copper Development Association — C65100 alloy record
Specification review
Technical verification requirements
Mechanical
Limited CDA temper/form coverage; no flat or annealed data.
Obtain producer data for the ordered form.
Grade selection
Phosphor and silicon bronzes — distinct grades
| Grade | Type | Key chemistry (limits) | Conductivity (CDA, 20°C) | Nearest EN / BS |
|---|---|---|---|---|
| C51000 | Wrought phosphor bronze | Sn 4.2–5.8%; P 0.03–0.35% | 15% IACS (5% Sn, 0.2% P basis) | Approx. CW451K CuSn5 / PB102 |
| C52100 | Wrought phosphor bronze | Sn 7.0–9.0%; P 0.03–0.35% | 13% IACS | Approx. CW453K CuSn8 / PB104 |
| PB1 | Cast phosphor bronze | Sn 10.0–11.5%; P 0.5–1.0% (EN 1982 CC481K casting) | Not stated as % IACS | Cross-referenced to CC481K CuSn11P-C |
| C65100 | Wrought low-silicon bronze | Si 0.8–2.0% | 12% IACS | Not CW116C |
| C65500 | Wrought high-silicon bronze | Si 2.8–3.8%; Mn 0.50–1.3% | 7% IACS | Related to CW116C CuSi3Mn1 / CS101 |
PB1 is a cast alloy and is not CW451K. UNS and EN chemistries differ, so “approximately” equivalent grades are not automatically cross-certified. Properties are never transferred between these grades.
Engineering reference
Technical data
| Element | Mass % |
|---|---|
| Silicon | 0.8–2.0 |
| Lead | 0.05 max |
| Zinc | 1.5 max |
| Iron | 0.8 max |
| Manganese | 0.7 max |
| Copper (incl. Ag) | Remainder |
| Cu + named elements | 99.5 min |
Copper Development Association — C65100 alloy record
| Property | Value | Basis |
|---|---|---|
| Density | 8.75 g/cm³ | From CDA specific gravity |
| Electrical conductivity | 12% IACS | 20°C |
| Thermal conductivity | 57.1 W/(m·K) | 20°C |
| Mean CTE 20–300°C | 17.8 × 10⁻⁶/K | Temper not stated |
| Elastic modulus (tension) | 117 GPa | Temperature not stated |
CDA generic values; temper, form and section not stated.
Copper Development Association — C65100 alloy record
Wire — H02 half hard
| Section | Tensile strength | Yield (0.5% extension) | Elongation | Hardness |
|---|---|---|---|---|
| 0.08 in (2.0 mm) | 80 ksi (552 MPa) | Not reported | 15% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C65100 alloy record
Wire — H04 hard
| Section | Tensile strength | Yield (0.5% extension) | Elongation | Hardness |
|---|---|---|---|---|
| 0.08 in (2.0 mm) | 100 ksi (690 MPa) | 70 ksi (483 MPa) | 11% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C65100 alloy record
Rod — H04 hard
| Section | Tensile strength | Yield (0.5% extension) | Elongation | Hardness |
|---|---|---|---|---|
| 1 in (25 mm) | 70 ksi (483 MPa) | 55 ksi (379 MPa) | 15% | Not reported |
CDA typical values at 20°C, not specification minima.
Copper Development Association — C65100 alloy record
Annealing range (CDA)
482–677°C (900–1250°F). Section, hold time and atmosphere are not stated; not a complete production schedule.
Temper designations
O60 soft anneal; H02 half hard; H04 hard; H08 spring. Grain-size anneals (OS) and O61 are separate tempers and are not relabelled.
Agree temper with the product specification.
Copper Development Association — C65100 alloy record
Typical applications
Engineering applications
- Fasteners
- Marine hardware
- Electrical hardware
- Chemical equipment
Subsequent manufacturing
Machining & processing
Cold working
Readily cold worked; strength depends strongly on form and temper.
Not heat-treatable
Strength comes from cold work (H tempers); annealing softens. Temper must be specified with the product form.
Application evidence
Listed applications are source-cited categories, not claims of stock or component approval.
Material certification & testing
Documentation must be agreed for the actual UNS/EN grade, product or casting specification, form, temper and section.
No certificate, approval or grade equivalence is automatic. “Nearest” or “related” designations do not certify compliance; quotation controls remain disabled.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Cast / lot traceability to the producing mill or foundry
- Chemical analysis and mechanical test results to the ordered specification
- Ultrasonic, impact or corrosion-related testing only where the ordered specification requires it
Material enquiry
Request a material quotation
C65100 Low-Silicon Bronze supplied to your material form, dimensions and specification.