Representative aluminium alloy plates with sawn edges

Materials Supply / Aluminium Alloys

Aluminium Alloy 5083

Non-heat-treatable Al-Mg-Mn | EN AW-5083 | Marine plate and profile tempers

Higher-magnesium, non-heat-treatable aluminium alloy used in demanding welded structures and marine environments, subject to specified temper and corrosion qualification.

Strength is controlled by chemistry, strain hardening, annealing and stabilisation where applicable, together with product form and thickness. These alloys are not strengthened by conventional solution heat treatment and precipitation ageing.

Illustrative aluminium sheet, plate and fabricated components; not certified alloy stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

Hulamin advertises H116/H321 plate 3–32 mm and H111 plate 3–60 mm; these supply ranges do not establish tensile-row thickness applicability. Hydro separately documents marine extrusions. ASTM B928 covers flat sheet/coiled sheet/plate only, not extrusions. Documented rolled-product forms only. Availability is subject to supplier, specification, temper and dimensional confirmation; no Quest stockholding is implied.

  • Marine plate
  • Sheet / coil (specification dependent)
  • Extruded marine profiles

Material overview

Aluminium Alloy 5083

Higher-magnesium, non-heat-treatable aluminium alloy used in demanding welded structures and marine environments, subject to specified temper and corrosion qualification.

  • Rolled marine plate and extruded profiles have separate conditions and references; sheet or plate values are never applied to bar or extrusions.
  • H116 and H321 are distinct corrosion-related tempers. Hulamin groups their published tensile minima; identical printed minima are not evidence of interchangeable processing, corrosion qualification or statistical behaviour.
  • Sensitisation and welded-joint performance require service- and product-specific assessment. No universal safe temperature, seawater immunity or pressure-equipment approval is asserted.

Designations and product specifications

Designations and product specifications
Designation / standardProduct / qualification scope
AA / EN AW5083 / EN AW-5083; Hydro independently lists the EN AW grade
UNS / European numerical numberNo primary registry or European numerical material number independently verified in this review; neither is asserted
ASTM B928/B928M-15(2023)e1High-Mg flat sheet, coiled sheet and plate for marine/similar environments; includes corrosion testing and identifiable inspection lots. Not an extrusion standard.
ASTM B209 / EN 485General rolled products; supplier lists do not demonstrate every marine acceptance requirement
ASTM G66-23 (ASSET)Exfoliation-susceptibility test; not a standalone marine material certificate
ASTM G67-24 (NAMLT)Nitric-acid mass-loss test for intergranular-corrosion susceptibility; acceptance criteria must come from the ordered product standard
EN 573-3 / EN 515Composition / temper terminology; current full requirements not accessed
EN 755 / EN 754 / EN 586Extruded / drawn / forged products need their own applicable requirements; plate data do not establish compliance
AMSNo applicable AMS product specification verified

Public scopes only; current full acceptance tables unavailable. Sources: https://www.astm.org/b0928_b0928m-15r23e01.html ; https://www.astm.org/g0066-23.html ; https://www.astm.org/g0067-24.html . Specify alloy, form, temper, thickness, testing and documentation; designation alone proves none of these.

ASTM B928/B928M-15(2023)e1 — high-magnesium marine sheet/plate (public scope)

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

  • H116/H321 marine acceptance

    Independent Hulamin brochure corroborates shared tensile minima, but does not establish ASTM G66/G67 test acceptance, lot sampling or gauge-specific requirements. H116 and H321 are not interchangeable processing routes.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

Grade selection

5052, 5083 and 5754 compared

5052, 5083 and 5754 compared
Aspect505250835754
Registered Mg range, mass %2.2–2.84.0–4.92.6–3.6
Other principal additionsCr 0.15–0.35%Mn 0.40–1.0%; Cr 0.05–0.25%Mn ≤0.50%; Cr ≤0.30%; Mn+Cr 0.10–0.60%
Metallurgical classificationNon-heat-treatable Al-Mg-CrNon-heat-treatable, higher-Mg Al-Mg-MnNon-heat-treatable Al-Mg
Conditions on these pagesO, H32, H34, H36, H38 sheet/coilO/H111/H112 extrusions; H111/H116/H321 plate (independent form-specific tables)O, H111, H22, H24, H26, H28 rolled products
Strength characteristicsCold work raises strength and reduces formabilityUsed for demanding welded structural plate; corrosion-qualified marine tempers require specific procurementStrength varies with cold work and partial annealing; not identical to 5052
FormabilityGood cold forming; softer tempers allow tighter bendsFormability depends on temper and thicknessSoft O/H111 suited to stamping and deep drawing
WeldabilityGood; strain-hardened HAZ may softenGood; parent, HAZ and weld-metal properties differExcellent producer rating; qualify joint properties
Corrosion and marine selectionGood seawater/atmospheric resistance, not immunityMarine plate requires appropriate temper and corrosion qualification; sensitisation is exposure dependentGood atmospheric and seawater resistance; not interchangeable with qualified 5083 plate
Documented product focusSheet and coilSheet/plate; confirm temper-specific availabilitySheet, strip/coil and plate

Qualitative selection guide. Chemistry from AA; fabrication from Vulcan/Hulamin/Gränges and the grade-specific references below. No numerical strength ranking: temper, form, thickness and test basis are not matched. No alloy is universally superior or automatically approved for marine, aerospace or pressure duty.

The Aluminum Association — Teal Sheets, December 2025 (registered composition limits)

Engineering reference

Technical data

Chemical composition limits — 5083 (AA)
ElementMass %Limit
Si0.40Maximum
Fe0.40Maximum
Cu0.10Maximum
Mn0.40–1.0Range
Mg4.0–4.9Range
Cr0.05–0.25Range
Zn0.25Maximum
Ti0.15Maximum
Other elements, each0.05Maximum
Other elements, total0.15Maximum
AlRemainderBalance

Registered wrought-alloy limits, not nominal values. Hulamin marine brochure prints Ti 0.25% maximum, conflicting with AA 0.15%; its chemistry is not merged into this table. Footnote 6 Be limit applies to welding electrode/rod/filler, not all plate. AA limits are not represented as an independently checked EN 573-3 table. Confirm the ordered specification and mill certificate.

The Aluminum Association — Teal Sheets, December 2025 (registered composition limits)

Physical properties — 5083 Hulamin reference values
PropertyValueBasis
Density2650 kg/m³Producer reference; AA calculated nominal is separately 2660 kg/m³
Elastic modulus71 GPaReference; temperature unspecified
Thermal conductivity117 W/(m·K)25°C; temper unspecified
Linear thermal expansion23.8 × 10⁻⁶ K⁻¹Interval unspecified
Melting range580–640°CNot a service-temperature limit

Producer values, not acceptance limits. Suspect electrical conductivity unit omitted pending producer clarification. Specific heat/resistivity not independently verified; no generic substitution from 5052 or 5754.

O extruded profiles — Hydro typical

O extruded profiles — Hydro typical
PropertyValue
Product thickness<25 mm
Ultimate tensile strength270 MPa
0.2% proof strength (Rp0.2)110 MPa
Elongation (source A min.)12%

Hydro Marine Standard Items: table heading says typical mechanical properties although elongation is labelled A min. Do not treat these as verified normative minima or design allowables. Orientation, tensile-test temperature, elongation gauge length and statistical basis not stated. Not rolled plate or bar data. Hydro MIG joint value is excluded because joint geometry/procedure/filler were insufficiently specified.

H112 extruded profiles — Hydro typical

H112 extruded profiles — Hydro typical
PropertyValue
Product thickness<25 mm
Ultimate tensile strength270 MPa
0.2% proof strength (Rp0.2)125 MPa
Elongation (source A min.)12%

Hydro Marine Standard Items: table heading says typical mechanical properties although elongation is labelled A min. Do not treat these as verified normative minima or design allowables. Orientation, tensile-test temperature, elongation gauge length and statistical basis not stated. Not rolled plate or bar data. Hydro MIG joint value is excluded because joint geometry/procedure/filler were insufficiently specified.

H111 extruded profiles — Hydro typical

H111 extruded profiles — Hydro typical
PropertyValue
Product thickness<25 mm
Ultimate tensile strength275 MPa
0.2% proof strength (Rp0.2)165 MPa
Elongation (source A min.)12%

Hydro Marine Standard Items: table heading says typical mechanical properties although elongation is labelled A min. Do not treat these as verified normative minima or design allowables. Orientation, tensile-test temperature, elongation gauge length and statistical basis not stated. Not rolled plate or bar data. Hydro MIG joint value is excluded because joint geometry/procedure/filler were insufficiently specified.

H111 marine plate — Hulamin published minima

H111 marine plate — Hulamin published minima
PropertyValue
Ultimate tensile strength≥275 MPa
Proof stress (offset not stated)≥125 MPa
Elongation≥15%

Hulamin producer brochure lists minima. Tensile-row thickness applicability, offset, orientation, temperature, gauge length and statistical basis not supplied. Advertised H111 3–60 mm / H116-H321 3–32 mm supply ranges are not guaranteed property ranges. H116 and H321 share one producer row, reproduced in distinct condition tables: no independent distribution or processing equivalence is claimed. Obtain thickness-specific mill/specification acceptance data before procurement.

H116 marine plate — Hulamin published minima

H116 marine plate — Hulamin published minima
PropertyValue
Ultimate tensile strength≥305 MPa
Proof stress (offset not stated)≥215 MPa
Elongation≥10%

Hulamin producer brochure lists minima. Tensile-row thickness applicability, offset, orientation, temperature, gauge length and statistical basis not supplied. Advertised H111 3–60 mm / H116-H321 3–32 mm supply ranges are not guaranteed property ranges. H116 and H321 share one producer row, reproduced in distinct condition tables: no independent distribution or processing equivalence is claimed. Obtain thickness-specific mill/specification acceptance data before procurement.

H321 marine plate — Hulamin published minima

H321 marine plate — Hulamin published minima
PropertyValue
Ultimate tensile strength≥305 MPa
Proof stress (offset not stated)≥215 MPa
Elongation≥10%

Hulamin producer brochure lists minima. Tensile-row thickness applicability, offset, orientation, temperature, gauge length and statistical basis not supplied. Advertised H111 3–60 mm / H116-H321 3–32 mm supply ranges are not guaranteed property ranges. H116 and H321 share one producer row, reproduced in distinct condition tables: no independent distribution or processing equivalence is claimed. Obtain thickness-specific mill/specification acceptance data before procurement.

O, H111 and H112

O is annealed. H111 describes slight strain hardening after annealing, such as levelling/straightening. H112 covers a limited work-hardened state with specified mechanical-property limits; neither implies conventional precipitation ageing. Profile and plate properties remain form-specific.

H116: corrosion-related strain-hardened condition

Historical H35.1 terminology describes strain hardening at the last operation to specified stable tensile limits, with accelerated intergranular/exfoliation corrosion requirements. Confirm the current ordered temper and product standard; this is not a generic quarter-hard designation.

H321: thermally stabilised corrosion-related condition

Historical H35.1 terminology describes thermal stabilisation after the last operation, with stable tensile limits and corrosion requirements. Matching tensile minima with H116 do not make the tempers interchangeable. Stabilisation is not precipitation strengthening.

Annealing, cold work and thermal exposure

No verified grade/form-specific producer annealing schedule was found, so no furnace temperature or holding time is prescribed. Annealing and weld heat can reduce strain-hardening strength; service exposure can sensitise higher-Mg material. No universal safe temperature is assigned.

Historical temper review is used for terminology only, not current contractual acceptance criteria. Obtain current H35.1/EN 515 and B928 requirements, mill process confirmation and corrosion evidence for the ordered product.

Material selection

Corrosion resistance & performance

Hulamin supports marine use, but 5083 is not immune to seawater pitting, crevice attack or galvanic corrosion. Environment, surface condition, drainage, dissimilar metals and protective finishes must be assessed for the actual structure.

Sensitisation involves grain-boundary β-Al3Mg2 (Mg2Al3) precipitation and preferential dissolution, increasing intergranular-corrosion and potentially intergranular stress-corrosion susceptibility. This does not usefully precipitation-harden 5083. Kinetics depend on temperature, duration and supplied microstructure/temper. Research reference: https://pmc.ncbi.nlm.nih.gov/articles/PMC5462825/ .

Published studies discuss sensitisation under prolonged exposure in roughly the 40–220°C range; these are research conditions, not an operating envelope. Cumulative time–temperature history, stress, environment and qualification matter. No universal indefinitely safe operating temperature or maximum service limit is claimed.

H116/H321 marine plate requires the applicable ordered corrosion qualification. ASTM G66 (ASSET) addresses exfoliation susceptibility and G67 (NAMLT) measures intergranular susceptibility by nitric acid mass loss. Test-method descriptions or alloy names are not evidence that an individual lot passes. No numerical B928 acceptance criteria are invented.

ASTM B928 addresses high-Mg marine flat products with corrosion testing and lot identification; it does not cover Hydro extrusions. Historical H321 requirements differed, so unspecified old stock cannot be assumed equivalent to current qualified material.

Assess welded regions separately from unaffected parent plate. No universal stress-corrosion immunity, cryogenic toughness or corrosion-life guarantee was verified. ASTM method references: https://www.astm.org/g0066-23.html ; https://www.astm.org/g0067-24.html .

Typical applications

Engineering applications

  • Marine structures and shipbuilding, where specified
  • Offshore fabricated equipment, subject to corrosion assessment
  • Welded tanks
  • Heavy-duty engineering fabrications
  • Pressure-containing structures only to applicable design/material specifications
  • Low-temperature storage equipment only with required design and material qualification

Subsequent manufacturing

Machining & processing

Welding: parent, HAZ, weld metal and joint

TWI explains that welding can remove work-hardening effects and soften the adjacent heat-affected zone. Unaffected parent material, unmelted HAZ, solidified weld metal and complete tested joint are different property bases. Parent-table values are not guaranteed joint strengths. Reference: https://www.twi-global.com/technical-knowledge/job-knowledge/weldability-of-materials-aluminium-alloys-021

Procedure and distortion control

Hulamin recommends 5183 preferentially and also lists 5356, but no filler is universally appropriate. Qualify filler, process, joint geometry, heat input, sequencing and inspection for the actual service. Control restraint and heat input to limit distortion; no numerical joint guarantee is given.

Forming and machining

Select bend radii, tooling, chip control and support by temper and section. No qualified alloy/temper-specific cutting parameters or universal forming radius were verified. Cold work changes condition and may affect corrosion response.

Cutting and surface finishing

Avoid contaminating aluminium surfaces, and assess coating/anodising and dissimilar-metal isolation with the intended marine or industrial environment. Confirm finish and dimensional inspection with the supplier.

Material certification & testing

Agree certification, temper, dimensions and inspection against the ordered material specification. Catalogue placement does not confer aerospace or pressure-equipment approval.

No test or certificate is automatically included. 5083 marine qualification must be evidenced for the ordered product, temper and specification; an alloy label alone is insufficient.

  • EN 10204 3.1 material certificate, where agreed
  • Certificate of Conformity
  • Heat / cast / batch traceability
  • Chemical analysis and temper verification
  • Mechanical testing and hardness testing where specified
  • For marine H116/H321 orders: obtain the applicable ordered product specification, lot traceability, mill certificate and required corrosion-test results; tensile results alone do not establish marine qualification.
  • Ultrasonic testing where applicable and agreed
  • Customer-specific inspection and acceptance requirements

Material enquiry

Request a material quotation

Aluminium Alloy 5083 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.