Representative aluminium alloy plates with sawn edges

Materials Supply / Aluminium Alloys

Aluminium Alloy 5754

Non-heat-treatable Al-Mg | EN AW-5754 / AlMg3 | UNS A95754 (secondary cross-reference)

Non-heat-treatable aluminium-magnesium alloy associated with European sheet and plate supply, offering good formability, weldability and corrosion resistance.

Strength is controlled by chemistry, strain hardening, annealing and stabilisation where applicable, together with product form and thickness. These alloys are not strengthened by conventional solution heat treatment and precipitation ageing.

Illustrative aluminium sheet, plate and fabricated components; not certified alloy stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

Documented rolled-product forms only. Availability is subject to supplier, specification, temper and dimensional confirmation; no Quest stockholding is implied.

  • Sheet
  • Plate
  • Coil / strip

Material overview

Aluminium Alloy 5754

Non-heat-treatable aluminium-magnesium alloy associated with European sheet and plate supply, offering good formability, weldability and corrosion resistance.

  • O and H111 are separate conditions even when a reference groups their mechanical limits. H22/H24/H26/H28 are strain hardened and partially annealed, not precipitation hardened.
  • Historic EN 485-2 rolled-product thickness bands are transcribed from a separately identified thyssenkrupp technical sheet; original Hulamin and Gränges literature corroborate O/H111 and H22.
  • Do not transfer thin-sheet elongation to thick plate or 5754 values to 5052. Branded automotive producer values are not generic EN minimums.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
AA / EN AW5754 / EN AW-5754 / EN AW-AlMg3
UNSA95754 — secondary Total Materia cross-reference; primary registry not inspected
DIN material number3.3535 in the thyssenkrupp sheet; historic DIN identifier, not a new EN number
EN 573-3Composition; source reproduces 2013-12 limits, not a current reviewed full standard
EN 485-2Sheet, strip and plate mechanical properties; tables below reproduce 2016-10 data in a 2017 sheet
EN 515Temper definitions; O, H111 and H2x meanings remain distinct
EN 754-2 / EN 755-2Cold-drawn / extruded products: separate specifications, not covered by rolled-product mechanical tables
ASTM B209/B209M5754 applicability is secondary cross-reference only; current full alloy/temper tables not accessed
AMS / EN 586No applicable aerospace AMS or forging specification verified

Current licensed ASTM/EN standard texts were unavailable. General EN rolled-product compliance does not confer special aerospace approval. Primary producer sources are Hulamin and Gränges; detailed H24/H26/H28 bands are a historic secondary table. UNS cross-reference: https://www.totalmateria.com/en-us/material/3018728

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

  • H26/H28 harder tempers

    Historic EN-based secondary limits do not establish current producer supply or qualification for harder tempers. Do not label absent producer data as contradicted values.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

Grade selection

5052, 5083 and 5754 compared

5052, 5083 and 5754 compared
Aspect505250835754
Registered Mg range, mass %2.2–2.84.0–4.92.6–3.6
Other principal additionsCr 0.15–0.35%Mn 0.40–1.0%; Cr 0.05–0.25%Mn ≤0.50%; Cr ≤0.30%; Mn+Cr 0.10–0.60%
Metallurgical classificationNon-heat-treatable Al-Mg-CrNon-heat-treatable, higher-Mg Al-Mg-MnNon-heat-treatable Al-Mg
Conditions on these pagesO, H32, H34, H36, H38 sheet/coilO/H111/H112 extrusions; H111/H116/H321 plate (independent form-specific tables)O, H111, H22, H24, H26, H28 rolled products
Strength characteristicsCold work raises strength and reduces formabilityUsed for demanding welded structural plate; corrosion-qualified marine tempers require specific procurementStrength varies with cold work and partial annealing; not identical to 5052
FormabilityGood cold forming; softer tempers allow tighter bendsFormability depends on temper and thicknessSoft O/H111 suited to stamping and deep drawing
WeldabilityGood; strain-hardened HAZ may softenGood; parent, HAZ and weld-metal properties differExcellent producer rating; qualify joint properties
Corrosion and marine selectionGood seawater/atmospheric resistance, not immunityMarine plate requires appropriate temper and corrosion qualification; sensitisation is exposure dependentGood atmospheric and seawater resistance; not interchangeable with qualified 5083 plate
Documented product focusSheet and coilSheet/plate; confirm temper-specific availabilitySheet, strip/coil and plate

Qualitative selection guide. Chemistry from AA; fabrication from Vulcan/Hulamin/Gränges and the grade-specific references below. No numerical strength ranking: temper, form, thickness and test basis are not matched. No alloy is universally superior or automatically approved for marine, aerospace or pressure duty.

The Aluminum Association — Teal Sheets, December 2025 (registered composition limits)

Engineering reference

Technical data

Chemical composition limits — 5754 (AA)
ElementMass %Limit
Si0.40Maximum
Fe0.40Maximum
Cu0.10Maximum
Mn0.50Maximum
Mg2.6–3.6Range
Cr0.30Maximum
Zn0.20Maximum
Ti0.15Maximum
Mn + Cr0.10–0.60Combined range
Other elements, each0.05Maximum
Other elements, total0.15Maximum
AlRemainderBalance

Registered wrought-alloy limits, not nominal values. The combined Mn+Cr range must be met as well as individual maxima. AA footnote 6 sets Be ≤0.0003% for welding electrode/rod/filler only, not a separate general sheet limit. AA limits are not represented as an independently checked EN 573-3 table. Confirm the ordered specification and mill certificate.

The Aluminum Association — Teal Sheets, December 2025 (registered composition limits)

Physical properties — 5754 Hulamin reference values
PropertyValue
Density2660 kg/m³
Elastic modulus68 GPa
Shear modulus26.5 GPa
Thermal conductivity147 W/(m·K)
Thermal expansion24 × 10⁻⁶ K⁻¹
Electrical resistivity49 nΩ·m
Melting interval595–645°C

Hulamin values only; no averaging with Novelis or thyssenkrupp. Measurement temperature and temper not specified; not guaranteed acceptance criteria. AA nominal density is separately 2670 kg/m³. Specific heat not verified and omitted. Melting range is not a service limit.

O sheet / strip / plate — historic EN table

O sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–0.5190–2408012% (A50)52
>0.5–1.5190–2408014% (A50)52
>1.5–3190–2408016% (A50)52
>3–12.5190–2408018% (A50)52
>12.5–100190–2408017% (A)52

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

H111 sheet / strip / plate — historic EN table

H111 sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–0.5190–2408012% (A50)52
>0.5–1.5190–2408014% (A50)52
>1.5–3190–2408016% (A50)52
>3–12.5190–2408018% (A50)52
>12.5–100190–2408017% (A)52

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

H22 sheet / strip / plate — historic EN table

H22 sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–0.5220–2701307% (A50)63
>0.5–1.5220–2701308% (A50)63
>1.5–3220–27013010% (A50)63
>3–6220–27013011% (A50)63
>6–12.5220–27013010% (A50)63
>12.5–40220–2701309% (A)63

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

H24 sheet / strip / plate — historic EN table

H24 sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–1.5240–2801606% (A50)70
>1.5–3240–2801607% (A50)70
>3–6240–2801608% (A50)70
>6–12.5240–28016010% (A50)70
>12.5–25240–2801608% (A)70

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

H26 sheet / strip / plate — historic EN table

H26 sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–1.5265–3051904% (A50)78
>1.5–3265–3051905% (A50)78
>3–6265–3051906% (A50)78

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

H28 sheet / strip / plate — historic EN table

H28 sheet / strip / plate — historic EN table
Thickness, mmUTS, MPaRp0.2 min, MPaElongation minHBW (information)
>0.2–1.5≥2902303% (A50)87
>1.5–3≥2902304% (A50)87

Room-temperature published limits/ranges reproduced by thyssenkrupp (2017), citing EN 485-2:2016-10; not current standard certification or statistical design allowables. Thickness lower bound exclusive, upper inclusive. Orientation unspecified. A50 and A retain distinct source gauge designations (A gauge basis not defined here). HBW is informational only, not an acceptance limit. Original Hulamin/Gränges support O/H111 and H22; detailed harder-temper bands require current mill/specification confirmation.

O and H111

O is annealed. H111 is annealed and slightly strain hardened by subsequent operations such as straightening; it is not simply an alternative label for O.

H22 / H24 / H26 / H28

Strain hardened and partially annealed to quarter-hard / half-hard / three-quarter-hard / fully hard. H1x denotes strain hardening only and H3x denotes stabilisation; equal strength limits do not make processing routes interchangeable.

Annealing and cold work

Novelis confirms cold forming and final annealing control strength. No original-producer numerical annealing schedule was verified, so no temperature or holding time is prescribed. Supplier heating-up times are not treated as soak times.

Welding, forming and stress relief

Cold forming changes strain-hardening state; annealing or weld heat can soften it. Select forming limits by thickness and temper, and confirm any stress relief/stabilisation route with the mill; do not introduce precipitation-ageing schedules.

Temper definitions from the cited EN 515-based producer supplement, not a rolled-product supply guarantee. Only separately supported O/H111 and H2x conditions are selected on this page.

Material selection

Corrosion resistance & performance

Hulamin rates corrosion resistance excellent, and thyssenkrupp supports atmospheric and seawater resistance. This does not establish universal immunity to chlorides, crevices, pitting or galvanic coupling. Qualify drainage, dissimilar-metal isolation and surface finishes for the environment.

Gränges supports marine-related and industrial applications. A producer IGC value without a named method/exposure is not represented as ASTM G67 qualification. No universal stress-corrosion or lifetime seawater guarantee is made.

5754 is not interchangeable with 5052 properties or 5083 corrosion-qualified marine plate. Protective finishing and service assessment depend on the assembled product.

Typical applications

Engineering applications

  • Automotive formed panels and components
  • Stamped and deep-drawn sheet components
  • Welded general engineering fabrications
  • Marine-related components, subject to specification
  • Food-industry components, subject to design and finish
  • European sheet and plate engineering applications

Subsequent manufacturing

Machining & processing

Forming

Gränges supports stamping and deep drawing in soft tempers. Hulamin shows higher bend radii in H22 than O/H111 for the same thickness; tooling and orientation still need qualification. Reference: https://www.granges.com/globalassets/03.-marknader-och-produkter/04.-granges-endure/granges-endure_data-sheet_5754.pdf

Welding and joints

Hulamin rates weldability excellent. Qualify process, filler, heat input and joint inspection for the ordered temper and section. Heat-affected-zone softening in strain-hardened material means parent-sheet limits are not guaranteed as-welded joint values. No numerical weld-metal or HAZ dataset is given.

Machining

Hulamin rates machinability fair; the secondary technical sheet warns of ribbon/thread chips in annealed material and reports improved machining after strain hardening. Use appropriate tooling and chip control, not a universal speed.

Cutting, finishing and distortion

Support thin sheet during cutting and joining; control weld sequencing, heat input and dimensional inspection. Qualify anodising/coatings for finish, corrosion and dimensional needs; no universal finish performance is promised.

Material certification & testing

Agree certification, temper, dimensions and inspection against the ordered material specification. Catalogue placement does not confer aerospace or pressure-equipment approval.

No test or certificate is automatically included. 5083 marine qualification must be evidenced for the ordered product, temper and specification; an alloy label alone is insufficient.

  • EN 10204 3.1 material certificate, where agreed
  • Certificate of Conformity
  • Heat / cast / batch traceability
  • Chemical analysis and temper verification
  • Mechanical testing and hardness testing where specified
  • Corrosion qualification testing where applicable (particularly 5083 H116/H321)
  • Ultrasonic testing where applicable and agreed
  • Customer-specific inspection and acceptance requirements

Material enquiry

Request a material quotation

Aluminium Alloy 5754 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.