Representative drawn pure copper round rods

Materials Supply / Copper & Copper-Base Alloys

C11000 Electrolytic Tough Pitch Copper (ETP)

ETP | UNS C11000 | Cu-ETP CW004A

C11000 contains oxygen as cuprous oxide. It has the same minimum annealed conductivity as C10200 but is susceptible to hydrogen embrittlement when heated in reducing atmospheres.

It must not be substituted for OF or OFE copper in hydrogen brazing, vacuum or reducing-atmosphere service.

Imagery is illustrative metal product forms, not certified C11000 stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

CDA lists flat products, rod/bar/shapes, forgings (B124), tube and wire. Confirm forms, sizes and availability at enquiry.

  • Sheet, strip and plate
  • Rod, bar and bus bar
  • Tube
  • Wire
  • Forgings

Material overview

C11000 Electrolytic Tough Pitch Copper (ETP)

The standard electrical copper: ≥99.90% Cu+Ag with a controlled oxygen content and 100% IACS minimum annealed conductivity.

  • CDA sets no oxygen maximum for the designation; Aurubis strip limits oxygen to 400 ppm.
  • A special low-oxygen Aurubis ETP wire claims hydrogen resistance; this is not generalised to conventional ETP.

Designations and specifications

Designations and specifications
Designation / standardScope and qualification
UNS / ENC11000; Cu-ETP, CW004A
ASTM B152 / B187 / B124Flat products / bus bar, rod and shapes / forging rod and bar
AMS 4500Soft-annealed sheet, strip and plate (CDA); current revision not verified
EN 13601 / EN 1652 / EN 12163Product families only; grade inclusion not verified

Copper Development Association — C11000 alloy record

Specification review

Technical verification requirements

  • Mechanical

    CDA does not report H02 yield strength for C11000.

    Obtain mill test data where yield is required.

  • Chemistry

    Oxygen content varies by producer; no designation limit.

    Specify oxygen limit if relevant.

Grade selection

C10100, C10200 and C11000 — distinct coppers

C10100, C10200 and C11000 — distinct coppers
AspectC10100 (OFE)C10200 (OF)C11000 (ETP)
TypeOxygen-free electronicOxygen-freeElectrolytic tough pitch (contains oxygen)
Copper (CDA designation)≥99.99% excl. Ag≥99.95% incl. Ag≥99.90% incl. Ag
Oxygen (CDA designation)≤5 ppm≤10 ppmNo limit in CDA designation; Aurubis strip ≤400 ppm
Individual impurity limits16 elements limitedNone in CDA designationNone in CDA designation
Min. conductivity, annealed, 20°C101% IACS100% IACS100% IACS
Hydrogen embrittlement in reducing atmospheresResistant to oxide-related mechanismResistant to oxide-related mechanismSusceptible

Designation limits are not product-specification acceptance requirements. ETP must not be substituted for OF/OFE where hydrogen brazing, vacuum or reducing-atmosphere service applies.

Copper Development Association — C10100 alloy record

Engineering reference

Technical data

Chemical composition
ElementCDA designationAurubis Cu-ETP strip
Copper + silver99.90% min99.90% min
OxygenNot limited in designation400 ppm max
BismuthNot limited5 ppm max
LeadNot limited50 ppm max

Aurubis values are producer limits for its strip product, not a universal C11000 oxygen limit.

Physical properties and conductivity — C11000
PropertyValueBasis
Electrical conductivity100% IACSAnnealed, 20°C — minimum
Thermal conductivity≈391 W/(m·K) (226 Btu/h·ft·°F)20°C; temper not stated
Density8.91 g/cm³ (0.322 lb/in³)20°C
Mean CTE 20–100°C16.9 × 10⁻⁶/K (9.4 × 10⁻⁶/°F)Temper not stated
Mean CTE 20–200°C17.3 × 10⁻⁶/K (9.6 × 10⁻⁶/°F)Temper not stated
Mean CTE 20–300°C17.6 × 10⁻⁶/K (9.8 × 10⁻⁶/°F)Temper not stated
Elastic modulus (tension)≈117 GPa (17,000 ksi)Temperature and temper not stated
Melting range1065–1083°CCDA

CDA values; metric figures converted from customary units. Cold work reduces conductivity slightly; confirm for the ordered temper. Aurubis strip datasheets report 127 GPa modulus — kept separate.

Copper Development Association — C11000 alloy record

OS050 annealed (0.050 mm grain) — flat, CDA typical

C11000 — OS050 annealed (0.050 mm grain) — flat, CDA typical
PropertyCDA typicalBasis
Tensile strength32 ksi (221 MPa)20°C; flat products, 0.040-in (1.0 mm) section
Yield strength (0.5% extension)10 ksi (69 MPa)Not an Rp0.2 value
Elongation45%Gauge length not stated

CDA typical values for this temper and section only, not specification minima.

Copper Development Association — C11000 alloy record

H02 half hard — flat, CDA typical

C11000 — H02 half hard — flat, CDA typical
PropertyCDA typicalBasis
Tensile strength42 ksi (290 MPa)20°C; flat products, 0.040-in (1.0 mm) section
Yield strength (0.5% extension)Not reportedNot an Rp0.2 value
Elongation14%Gauge length not stated

CDA typical values for this temper and section only, not specification minima.

Copper Development Association — C11000 alloy record

H04 hard — flat, CDA typical

C11000 — H04 hard — flat, CDA typical
PropertyCDA typicalBasis
Tensile strength50 ksi (345 MPa)20°C; flat products, 0.040-in (1.0 mm) section
Yield strength (0.5% extension)45 ksi (310 MPa)Not an Rp0.2 value
Elongation6%Gauge length not stated

CDA typical values for this temper and section only, not specification minima.

Copper Development Association — C11000 alloy record

Not heat-treatable

These coppers are strengthened only by cold work (H tempers) and softened by annealing (O / OS tempers).

Reducing atmospheres

ETP (C11000) reacts with hydrogen at elevated temperature: hydrogen combines with internal cuprous oxide forming steam and causing embrittlement. OF and OFE resist this oxide-related mechanism.

Oxide test

ASTM B577 is a test method for cuprous oxide in oxygen-free and deoxidised copper; ASTM B170 Grade 1 (C10100) requires ten reverse bends and Grade 2 (C10200) eight after B577 Method D.

No specific annealing temperatures are given here; agree temper with the product specification.

ASTM B577 — official listing

Typical applications

Engineering applications

  • General electrical conductors and bus bars
  • Transformer and switchgear components
  • Electronic components not exposed to reducing atmospheres

Subsequent manufacturing

Machining & processing

Brazing and vacuum use

Select OF or OFE for hydrogen brazing, vacuum electronics and reducing atmospheres; ETP is not suitable for these conditions.

Forming

All three cold-form readily; strength rises and conductivity falls slightly with cold work.

Application evidence

Listed applications are source-cited categories, not claims of stock or component approval.

Material certification & testing

Documentation must be agreed for the actual UNS/EN grade, product specification, form, temper and any conductivity or oxygen-content test.

No certificate, conductivity guarantee, approval or grade equivalence is automatic; quotation controls remain disabled.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Cast / lot traceability to the producing mill
  • Chemical analysis, including oxygen where specified
  • Electrical conductivity and mechanical test results for the supplied temper, where ordered

Material enquiry

Request a material quotation

C11000 Electrolytic Tough Pitch Copper (ETP) supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.