Materials Supply / Nickel, Cobalt & High-Temperature Alloys
Hastelloy X Nickel Superalloy
Nickel-chromium-iron-molybdenum alloy | UNS N06002 | W.Nr. 2.4665
Hastelloy X is a nickel-chromium-iron-molybdenum alloy for gas-turbine, furnace and chemical-process components.
AMS 5754 covers bars, forgings, flash-welded rings and stock for forging, flash-welded rings or heading. AMS 5587 covers seamless tubing. These are not interchangeable: machining a bore in AMS 5754 bar or forging stock does not establish AMS 5587 tube conformity. Order the required product specification and verify manufacturing route, heat treatment, inspection, testing and certification.
HASTELLOY® is a trademark of Haynes International, Inc. Quest Engineering does not own the trademark or manufacture the alloy.
Raw & semi-finished materials
Available material forms
Producer-supported product forms; availability is subject to ordered specification, dimensions and supplier confirmation. No Quest Engineering stockholding is implied.
- Plate
- Sheet
- Strip
- Bar
- Billet
- Forgings
- Seamless pipe and tube
- Welded pipe and tube
- Fittings
- Welding wire
Material overview
Hastelloy X Nickel Superalloy
Oxidation-resistant nickel superalloy combining high-temperature strength with forming and welding capability.
- AMS 5754 covers bars, forgings, flash-welded rings and stock for forging, flash-welded rings or heading. AMS 5587 covers seamless tubing. These are not interchangeable: machining a bore in AMS 5754 bar or forging stock does not establish AMS 5587 tube conformity. Order the required product specification and verify manufacturing route, heat treatment, inspection, testing and certification.
- Published typical properties must not be substituted for ordered specification requirements. No graph-derived values or invented acceptance limits are included.
Material specifications and designations
| Designation / standard | Product scope / qualification |
|---|---|
| UNS | N06002 |
| W.Nr. / DIN | 2.4665 / NiCr22Fe18Mo |
| AMS 5754P | Bars, forgings, flash-welded rings and forging/ring/heading stock; solution heat treated — SAE public Scope |
| AMS 5587G | Seamless tubing; solution heat treated — SAE public Scope |
| AMS 5536 | Sheet, plate and strip — Haynes listing |
| ASTM B435 / ASME SB435 | Sheet, plate and strip — Haynes listing |
| ASTM B572 / ASME SB572; ASTM B472 | Billet, rod and bar heading — Haynes listing; individual scope requires ordered standard |
| ASTM B622 / ASME SB622 | Seamless pipe and tube — Haynes listing |
| ASTM B619 / ASME SB619; ASTM B626 / ASME SB626 | Welded pipe / tube — Haynes listing |
| ASTM B366 / ASME SB366 | Fittings — Haynes listing |
| AMS 5588 | Welded pipe and tube heading — Haynes listing; not AMS 5587 |
AMS 5754 covers bars, forgings, flash-welded rings and stock for forging, flash-welded rings or heading. AMS 5587 covers seamless tubing. These are not interchangeable: machining a bore in AMS 5754 bar or forging stock does not establish AMS 5587 tube conformity. Order the required product specification and verify manufacturing route, heat treatment, inspection, testing and certification. SAE scopes: https://saemobilus.sae.org/standards/ams5754p-nickel-alloy-corrosion-heat-resistant-bars-forgings-rings-forging-ring-heading-stock-475ni-22cr-15co-90mo-060w-185fe-alloy-x-solution-heat-treated ; https://saemobilus.sae.org/standards/ams5587g-nickel-alloy-corrosion-heat-resistant-seamless-tubing-475ni-22cr-15co-90mo-060w-185fe-solution-heat-treated. Standard listings are not blanket equivalence or certification. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.
Specification review
Technical verification requirements
Specifications / product form
Producer listings and historic references support alloy association but not every listed standard’s current revision, individual form, section-size, melt-route, heat-treatment tolerances or acceptance requirements. Existing qualification wording is appropriate, not proof of conformity.
Obtain controlled ordered-standard and producer confirmation before technical release.
AMS 5754 versus AMS 5587
Current page correctly separates bar/forging from seamless tubing. Accessed H-3009E supports AMS5754 for billet/bar and forgings but does not establish the page’s AMS5587G revision and full scope. Do not report the historic target as a confirmed present interchangeability defect.
Check official SAE scope and ordered full revisions for 5754 and 5587 before release; retain form distinction.
Engineering reference
Technical data
| Element | Mass % | Meaning |
|---|---|---|
| Nickel | 47; balance | Nominal / balance |
| Chromium | 22 | Nominal |
| Iron | 18 | Nominal |
| Molybdenum | 9 | Nominal |
| Cobalt | 1.5 | Nominal |
| Tungsten | 0.6 | Nominal |
| Carbon | 0.1 | Nominal |
| Manganese | 1 | Maximum explicitly printed in nominal table |
| Silicon | 1 | Maximum explicitly printed in nominal table |
| Boron | 0.008 | Maximum explicitly printed in nominal table |
| Niobium | 0.5 | Maximum explicitly printed in nominal table |
| Aluminum | 0.5 | Maximum explicitly printed in nominal table |
| Titanium | 0.15 | Maximum explicitly printed in nominal table |
Nominal chemistry, not a complete controlled specification-limits table. Only explicitly marked maxima are maxima; nominal values must not be presented as identical minimum/maximum limits. Outstanding: a complete controlled chemistry-limits table applicable to the ordered wrought product and revision has not been verified from a single accessible SAE/ASTM or producer source. Do not use this nominal panel for chemical acceptance.
| Property | Temperature / interval °C | Value | Unit |
|---|---|---|---|
| Density | 22 | 8220 | kg/m³ |
| Melting range | — | 1260–1355 | °C |
| Specific heat | RT | 486 | J/(kg·K) |
| Poisson ratio | 22 | 0.32 | — |
| Relative magnetic permeability | RT; 15900 A/m | 1.002 | — |
| Thermal conductivity | 25 | 9.2 | W/(m·K) |
| Thermal conductivity | 100 | 11.2 | W/(m·K) |
| Thermal conductivity | 200 | 14.1 | W/(m·K) |
| Thermal conductivity | 600 | 20.9 | W/(m·K) |
| Thermal conductivity | 650 | 21.9 | W/(m·K) |
| Thermal conductivity | 700 | 22.8 | W/(m·K) |
| Thermal conductivity | 750 | 23.8 | W/(m·K) |
| Thermal conductivity | 800 | 24.7 | W/(m·K) |
| Thermal conductivity | 850 | 25.7 | W/(m·K) |
| Thermal conductivity | 900 | 26.7 | W/(m·K) |
| Specific heat | 100 | 487 | J/(kg·K) |
| Specific heat | 200 | 484 | J/(kg·K) |
| Specific heat | 300 | 491 | J/(kg·K) |
| Specific heat | 400 | 507 | J/(kg·K) |
| Specific heat | 500 | 531 | J/(kg·K) |
| Specific heat | 600 | 564 | J/(kg·K) |
| Specific heat | 700 | 606 | J/(kg·K) |
| Specific heat | 800 | 657 | J/(kg·K) |
| Specific heat | 900 | 716 | J/(kg·K) |
| Specific heat | 1000 | 784 | J/(kg·K) |
| Dynamic elastic modulus | RT | 205 | GPa |
| Dynamic elastic modulus | 100 | 202 | GPa |
| Dynamic elastic modulus | 200 | 198 | GPa |
| Dynamic elastic modulus | 300 | 192 | GPa |
| Dynamic elastic modulus | 400 | 187 | GPa |
| Dynamic elastic modulus | 500 | 180 | GPa |
| Dynamic elastic modulus | 600 | 173 | GPa |
| Dynamic elastic modulus | 700 | 165 | GPa |
| Dynamic elastic modulus | 800 | 157 | GPa |
| Dynamic elastic modulus | 900 | 148 | GPa |
| Mean thermal expansion | 26–100 | 13.9 | 10⁻⁶/K |
| Mean thermal expansion | 26–500 | 15 | 10⁻⁶/K |
| Mean thermal expansion | 26–600 | 15.3 | 10⁻⁶/K |
| Mean thermal expansion | 26–700 | 15.7 | 10⁻⁶/K |
| Mean thermal expansion | 26–750 | 15.9 | 10⁻⁶/K |
| Mean thermal expansion | 26–800 | 16 | 10⁻⁶/K |
| Mean thermal expansion | 26–850 | 16.2 | 10⁻⁶/K |
| Mean thermal expansion | 26–900 | 16.4 | 10⁻⁶/K |
| Mean thermal expansion | 26–975 | 16.6 | 10⁻⁶/K |
Density converted exactly from 8.22 g/cm³. RT means room temperature; no exact RT assigned when not given. Electrical-resistivity column has an apparent unit/conversion inconsistency and is excluded pending producer clarification. Remaining metric entries are the producer’s printed metric-column values, not recalculated conversions of the adjacent British column; those columns can use different temperature grids. Replacing °C temperature-difference units with K changes no numerical conductivity, specific-heat or expansion value. Mean expansion is an interval average, not an instantaneous coefficient. Dynamic modulus is not relabelled static modulus. The density conversion is 8.22 × 1000 = 8220 kg/m³. Source precision is retained, not a claim of exact measured properties.
Solution-annealed plate
| Property | Value | Basis |
|---|---|---|
| Ultimate tensile strength | 760 MPa | 21°C; producer typical tensile data |
| 0.2% yield strength | 340 MPa | 21°C; producer typical tensile data |
| Elongation | 48.9 % | 21°C; gauge length not stated in this table |
| Hardness | 87 HRB | Separate room-temperature hardness table; solution annealed at 2150°F (1177°C) |
| Reduction of area | Not tabulated | Not reported in the cited room-temperature plate/sheet tensile tables; no value inferred. |
Indicative producer test results, not specification minima. Hardness is from a separate table, not the tensile specimens. No hardness conversion or acceptance limit inferred. Hardness condition is explicit in the source heading: “Room Temperature Hardness of Material Solution Annealed at 2150°F”: sheet 86 HRB; plate 87 HRB. The tensile table itself does not repeat a solution-treatment schedule; its solution-treated description follows the brochure’s general wrought-supply condition, not specimen-specific heat-treatment documentation. Do not claim a matched heat, lot or test specimen. Typical producer values, not specification minima or design allowables; confirm ordered condition, section limits, specimen requirements and gauge length where not stated.
Solution-annealed sheet
| Property | Value | Basis |
|---|---|---|
| Ultimate tensile strength | 783 MPa | 21°C; producer typical tensile data |
| 0.2% yield strength | 376 MPa | 21°C; producer typical tensile data |
| Elongation | 46.5 % | 21°C; gauge length not stated in this table |
| Hardness | 86 HRB | Separate room-temperature hardness table; solution annealed at 2150°F (1177°C) |
| Reduction of area | Not tabulated | Not reported in the cited room-temperature plate/sheet tensile tables; no value inferred. |
Indicative producer test results, not specification minima. Hardness is from a separate table, not the tensile specimens. No hardness conversion or acceptance limit inferred. Hardness condition is explicit in the source heading: “Room Temperature Hardness of Material Solution Annealed at 2150°F”: sheet 86 HRB; plate 87 HRB. The tensile table itself does not repeat a solution-treatment schedule; its solution-treated description follows the brochure’s general wrought-supply condition, not specimen-specific heat-treatment documentation. Do not claim a matched heat, lot or test specimen. Typical producer values, not specification minima or design allowables; confirm ordered condition, section limits, specimen requirements and gauge length where not stated.
Product-form-specific producer test data, not specification minima or design allowables.
Tensile data — plate
| Test temperature °C | UTS MPa | 0.2% yield MPa | Elongation % |
|---|---|---|---|
| 21 | 760 | 340 | 48.9 |
| 538 | 604 | 224 | 60.2 |
| 649 | 558 | 212 | 63.5 |
| 760 | 421 | 218 | 74.5 |
| 871 | 255 | 189 | 98.1 |
| 982 | 138 | 94 | 98.1 |
| 1093 | 72 | 45 | 95.3 |
Producer typical data for solution-treated wrought product; not guaranteed minima, not design allowables. Gauge length not stated.
Tensile data — sheet
| Test temperature °C | UTS MPa | 0.2% yield MPa | Elongation % |
|---|---|---|---|
| 21 | 783 | 376 | 46.5 |
| 538 | 628 | 253 | 53.6 |
| 649 | 580 | 241 | 65.5 |
| 760 | 424 | 233 | 95.6 |
| 871 | 251 | 193 | 117.9 |
| 982 | 130 | 88 | 81.5 |
| 1093 | 65 | 43 | 50.6 |
Producer typical data for solution-treated wrought product; not guaranteed minima, not design allowables. Gauge length not stated.
Creep and rupture — solution-annealed plate
| Temperature °C | Creep % / R=rupture | 10 h MPa | 100 h MPa | 1000 h MPa | 10000 h MPa |
|---|---|---|---|---|---|
| 649 | 0.5 | - | 188 | 128 | 88 |
| 649 | 1 | - | 207 | 145 | 107 |
| 704 | 0.5 | 172 | 112 | 77 | 57 |
| 704 | 1 | 186 | 131 | 97 | 72 |
| 704 | R | 317 | 221 | 159 | 117 |
| 760 | 0.5 | 103 | 71 | 52 | 39 |
| 760 | 1 | 124 | 90 | 66 | 49 |
| 760 | R | 207 | 146 | 107 | 79 |
| 816 | 0.5 | 68 | 50 | 37 | 27 |
| 816 | 1 | 86 | 63 | 46 | 32 |
| 816 | R | 141 | 103 | 72 | 50 |
| 871 | 0.5 | 48 | 35 | 26 | 17 |
| 871 | 1 | 61 | 44 | 31 | 20 |
| 871 | R | 100 | 69 | 47 | 31 |
| 927 | 0.5 | 35 | 25 | 16 | 9 |
| 927 | 1 | 44 | 30 | 19 | 10 |
| 927 | R | 69 | 46 | 30 | 18 |
| 982 | 0.5 | 25 | 16 | 8.6 | 3.8 |
| 982 | 1 | 30 | 19 | 10 | 4.5 |
| 982 | R | 46 | 30 | 18 | 10 |
| 1038 | 0.5 | 16 | 9 | 3.8 | - |
| 1038 | 1 | 19 | 10 | 4.5 | - |
| 1038 | R | 30 | 18 | 10 | - |
Approximate initial stress to produce specified creep or rupture. * Significant extrapolation. — / - means not tabulated, not zero. Printed SI values retained even where imperial conversion differs. Not allowable stresses.
Creep and rupture — solution-annealed sheet
| Temperature °C | Creep % / R=rupture | 10 h MPa | 100 h MPa | 1000 h MPa | 10000 h MPa |
|---|---|---|---|---|---|
| 649 | 0.5 | - | 178 | 124 | - |
| 649 | 1 | - | 193 | 145 | - |
| 704 | 0.5 | 162 | 112 | 83 | - |
| 704 | 1 | 179 | 131 | 97 | - |
| 704 | R | 303 | 221 | 159 | 117 |
| 760 | 0.5 | 103 | 76 | 56 | - |
| 760 | 1 | 124 | 90 | 66 | 49 |
| 760 | R | 207 | 146 | 107 | 79 |
| 816 | 0.5 | 72 | 53 | 37 | - |
| 816 | 1 | 86 | 63 | 45 | 30 |
| 816 | R | 141 | 103 | 72 | 50 |
| 871 | 0.5 | 52 | 35 | 22 | - |
| 871 | 1 | 61 | 43 | 27 | 16 |
| 871 | R | 100 | 69 | 47 | 29 |
| 927 | 0.5 | 35 | 21 | 11 | - |
| 927 | R | 69 | 46 | 28 | 17 |
| 982 | 0.5 | 21 | 11 | 3.3 | - |
| 982 | R | 46 | 28 | 16 | 8.3 |
| 1038 | 0.5 | 11 | - | - | - |
| 1038 | R | 28 | 17 | 8.3 | - |
| 1093 | 0.5 | 4.3 | - | - | - |
| 1093 | R | 17 | 8.6 | 2.8 | - |
Approximate initial stress to produce specified creep or rupture. * Significant extrapolation. — / - means not tabulated, not zero. Printed SI values retained even where imperial conversion differs. Not allowable stresses.
Static oxidation — flowing air, 1008 hours
| Temperature °C (as printed) | Metal loss per side mm | Metal loss + CIP per side mm |
|---|---|---|
| 980 | 0.007 | 0.019 |
| 1095 | 0.038 | 0.069 |
Cycled to room temperature once weekly. CIP = continuous internal penetration. Results are test-specific, not universal service-temperature limits.
Oxidation performance
- Strong oxidation resistance is a principal feature; oxidation tests do not establish a universal continuous-use limit.
Exposure time, atmosphere, stress and thermal cycling govern suitability. No values estimated from graphs. Suitability depends on loading, temperature, atmosphere, exposure duration and required service life. Test temperatures are not universal maximum service temperatures.
Solution heat treatment
Typically 2150°F (1177°C), followed by rapid cooling. Bright-annealed products are cooled in hydrogen.
After forming
Anneal and rapidly cool hot- or cold-worked parts to restore the best balance of properties.
Wrought forms are supplied solution heat treated unless otherwise specified. Lower-temperature anneals can precipitate secondary phases and affect strength and ductility. No universal hold time or cooling rate is specified. The producer prints 2150°F (1177°C); the arithmetic conversion is 1176.666…°C, rounded to 1177°C. This is a typical treatment, not a specification acceptance tolerance; no time-at-temperature requirement is invented.
Material selection
Corrosion resistance & performance
Haynes reports exceptional resistance to stress-corrosion cracking in petrochemical applications; this is not a universal immunity claim.
Oxidation, carburization and hot corrosion are distinct mechanisms; validate against the actual process environment.
Typical applications
Engineering applications
- Gas-turbine transition ducts, combustor cans, spray bars and flame holders
- Afterburners, tailpipes and cabin heaters
- Furnace rolls, retorts, muffles, catalyst support grids and baffles
- Pyrolysis tubing and flash-drier components
Subsequent manufacturing
Machining & processing
Hot and cold forming
For hot working, hold at 2150°F (1177°C) long enough to bring the whole piece to temperature. Readily cold formed; anneal and rapidly cool after working.
Welding
GTAW, GMAW, SMAW and resistance welding are supported. Submerged arc welding is not recommended because high heat input and slow cooling can promote cracking. Thoroughly clean weld surfaces.
Machining and product conformity
AMS 5754 covers bars, forgings, flash-welded rings and stock for forging, flash-welded rings or heading. AMS 5587 covers seamless tubing. These are not interchangeable: machining a bore in AMS 5754 bar or forging stock does not establish AMS 5587 tube conformity. Order the required product specification and verify manufacturing route, heat treatment, inspection, testing and certification.
Machining condition and tooling
Confirm the actual material condition before planning machining. Allow for work hardening; qualify tool material, rigidity, coolant and cutting engagement for the product. No universal speeds or feeds are specified.
Distortion, finishing and inspection
Agree machining allowance, final surface condition and dimensional inspection around heat treatment. Define surface and internal inspection, acceptance criteria and traceability to the ordered specification; additional testing is not automatic.
Material certification & testing
Certification and inspection options are subject to customer requirements and supplier confirmation.
Conformity must be demonstrated against the ordered specification, form and condition. Tests are not automatic; agree scope, acceptance criteria and documentation before ordering.
- EN 10204 3.1 material certificates
- Certificates of Conformity
- Heat/batch traceability
- Chemical analysis
- Mechanical testing
- Heat-treatment records
- Hardness testing
- Positive Material Identification (PMI)
- Ultrasonic testing where applicable
- Additional aerospace or customer-specific inspection requirements
Material enquiry
Request a material quotation