Representative ground nickel-based alloy round bars

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

Inconel 617 Nickel Alloy

Solid-solution-strengthened nickel-chromium-cobalt-molybdenum alloy | UNS N06617 | W.Nr. 2.4663

Inconel 617 is a nickel-chromium-cobalt-molybdenum alloy strengthened principally by cobalt and molybdenum in solid solution. Chromium and aluminium support protective oxide formation; mechanical performance and environmental resistance must be assessed separately.

Normally used solution annealed, the alloy is employed in gas-turbine combustion hardware, heat-treatment equipment and selected power-generation components. Grain size, residual cold work and prolonged thermal exposure can affect creep and fatigue behaviour.

INCONEL® is a trademark of the Special Metals Corporation group of companies, as stated in the producer bulletin. Quest Engineering does not own this trademark.

Raw & semi-finished materials

Available material forms

Producer-listed product families only. Availability depends on specification, dimensions and supplier confirmation; no Quest Engineering stock is implied. Confirm tube manufacturing route separately.

  • Rod and Bar
  • Wire
  • Forging Stock
  • Forgings and Rings
  • Plate
  • Sheet
  • Strip
  • Pipe
  • Tube
  • Cut-to-Size Material

Material overview

Inconel 617 Nickel Alloy

A solid-solution-strengthened nickel alloy combining elevated-temperature strength, creep resistance and oxidation resistance for demanding thermal service.

  • Solid-solution strengthening supports elevated-temperature strength without an Inconel 718-type ageing cycle.
  • Solution annealing and controlled grain size balance creep strength, ductility and fatigue performance.
  • Good metallurgical stability does not mean properties remain unchanged: prolonged exposure can cause carbide and gamma-prime precipitation.
  • Technical values are producer reference data, not design allowables or proof of conformity to an ordered specification.

Material specifications & designations

Material specifications & designations
Designation / specificationProduct form / scopeNotes
UNS N06617Parent alloy identificationProducer designation; not a product acceptance specification.
DIN EN material designation (VDM producer reference)2.4663 — NiCr23Co12MoVDM Alloy 617, July 2021, p. 2, Table 1; UNS N06617. Producer designation association, not proof of interchangeable product requirements. The Special Metals March 2005 bulletin prints 2.4663a; the unexplained trailing a is not adopted as the ordering identifier.
ASTM B166Rod, bar and wirePublic B166-08 abstract includes N06617: hot-finished/cold-worked rounds, squares, hexagons, rectangles and cold-worked wire. Condition and limits depend on order.
ASTM B168Rolled plate, sheet and stripN06617 verified in public B168-19e1 abstract; not bar or tubing.
ASTM B564Nickel-alloy forgingsN06617 included in public B564-06 scope; not a blanket forging-stock acceptance standard.
ASTM B546Electric fusion-welded pipePublic B546-19(2024) abstract includes N06617; annealed, full-penetration double-welded joints with filler. Not seamless pipe/tube.
AMS 5887Bars, forgings, flash-welded rings; forging/ring stockSAE AMS5887F public scope: products under 102 mm least cross-sectional dimension; stock of any size for forging or flash-welded rings. Annealed; specified melting route.
AMS 5888PlateSAE AMS5888E public scope: nominal thickness 50.8 mm and under, inclusive; annealed, specified melting route.
AMS 5889Sheet and stripProducer association; AMS5889D public distributor abstract confirms form and annealed title; direct SAE abstract not retrieved.
EN product specificationNot independently establishedNo EN product-standard equivalence claimed. Bulletin lists legacy DIN and VdTÜV references; current status and equivalence require confirmation.

Each entry is separate and form-specific. Full current ASTM/AMS texts were not accessible; abstracts do not verify all chemistry, condition, dimensional or testing requirements. Bulletin also lists ASME SB166, SB168, SB564 and SB546; applicable Code edition must be checked independently. AWS A5.14/ERNiCrCoMo-1 and AWS A5.11/ENiCrCoMo-1 are welding consumables, not parent-metal specifications. Public abstract URLs and checked revisions are recorded in the accompanying notes.

Specification review

Technical verification requirements

  • Designations / ordered product condition

    Literal 2.4663a identifier conflicts with VDM 2.4663; establish whether the trailing a is a typographical/annotation artefact before ordering. Existing cautions do not prove conformity; no allegation that every listed scope is wrong. Obtain the ordered revision and map each cited specification to form, dimensions, manufacture, delivery condition and acceptance tests.

    Obtain licensed ordered editions and issue a material-specific form/condition/size compliance matrix; retain existing caveats pending approval.

Engineering reference

Technical data

Chemical composition
ElementMass %
Nickel44.5 min.
Chromium20.0–24.0
Cobalt10.0–15.0
Molybdenum8.0–10.0
Aluminium0.8–1.5
Carbon0.05–0.15
Iron3.0 max.
Manganese1.0 max.
Silicon1.0 max.
Sulfur0.015 max.
Titanium0.6 max.
Copper0.5 max.
Boron0.006 max.

Special Metals SMC-029, March 2005, p. 1 Table 1: producer limiting chemical composition, mass %. These are producer-reported limits, not typical or nominal measured chemistry and not independently verified current ASTM/AMS acceptance limits. No phosphorus, niobium or tantalum limit is given in this table; none is imported from VDM or another specification. Confirm contractual chemistry against the ordered product specification and revision.

Physical properties
PropertyValueTemperature / basis
Density8360 kg/m³Room temperature; Table 2 gives 8.36 Mg/m³
Melting range1332–1380 °CTable 2
Specific heat419 J/(kg·K)26 °C, Table 2
Electrical resistivity1.22 µΩ·m26 °C, Table 2
Thermal conductivity13.4; 20.9; 28.7 W/(m·K)20; 500; 1000 °C respectively, Table 3
Specific heat419; 536; 662 J/(kg·K)20; 500; 1000 °C respectively, Table 3
Electrical resistivity1.222; 1.290; 1.378 µΩ·m20; 500; 1000 °C respectively, Table 3
Mean linear thermal expansion11.6; 13.9; 16.3 × 10⁻⁶ K⁻¹26–100; 26–500; 26–1000 °C respectively
Tensile elastic modulus211; 181; 139; 129 GPa25; 500; 1000; 1100 °C respectively, Table 4
Shear modulus81; 70; 53; 49 GPa25; 500; 1000; 1100 °C respectively, Table 4

Typical reference properties, not specification limits. Table 3 conductivity is calculated from resistivity and specific heat is calculated. CTE is mean from 26 °C to stated temperature. Table 3 SI baseline is printed as 20 °C whereas Table 2 constants use 26 °C; these are retained separately. Moduli measured dynamically.

Solution annealed — hot-rolled plate

Room-temperature mechanical properties — solution-annealed hot-rolled plate
PropertyValueBasis
Ultimate tensile strength734 MPaTypical
0.2% yield strength322 MPaTypical
Elongation62%Typical; gauge length not stated
Hardness172 BHNProducer Brinell notation
Reduction of area56%Typical

Table 5, page 3: typical room-temperature values, not specification minima. Production method precedes solution annealing. Plate/sheet/strip tests are transverse. Section dimensions, gauge length and bar/tube orientation are not stated; do not extrapolate to all sizes. Reduction of area is not reported for tubing or sheet/strip.

Solution annealed — hot-rolled bar

Room-temperature mechanical properties — solution-annealed hot-rolled bar
PropertyValueBasis
Ultimate tensile strength769 MPaTypical
0.2% yield strength318 MPaTypical
Elongation56%Typical; gauge length not stated
Hardness181 BHNProducer Brinell notation
Reduction of area50%Typical

Table 5, page 3: typical room-temperature values, not specification minima. Production method precedes solution annealing. Plate/sheet/strip tests are transverse. Section dimensions, gauge length and bar/tube orientation are not stated; do not extrapolate to all sizes. Reduction of area is not reported for tubing or sheet/strip.

Solution annealed — cold-drawn tubing

Room-temperature mechanical properties — solution-annealed cold-drawn tubing
PropertyValueBasis
Ultimate tensile strength758 MPaTypical
0.2% yield strength383 MPaTypical
Elongation56%Typical; gauge length not stated
Hardness193 BHNProducer Brinell notation

Table 5, page 3: typical room-temperature values, not specification minima. Production method precedes solution annealing. Plate/sheet/strip tests are transverse. Section dimensions, gauge length and bar/tube orientation are not stated; do not extrapolate to all sizes. Reduction of area is not reported for tubing or sheet/strip.

Solution annealed — cold-rolled sheet or strip

Room-temperature mechanical properties — solution-annealed cold-rolled sheet or strip
PropertyValueBasis
Ultimate tensile strength755 MPaTypical
0.2% yield strength351 MPaTypical
Elongation58%Typical; gauge length not stated
Hardness173 BHNProducer Brinell notation

Table 5, page 3: typical room-temperature values, not specification minima. Production method precedes solution annealing. Plate/sheet/strip tests are transverse. Section dimensions, gauge length and bar/tube orientation are not stated; do not extrapolate to all sizes. Reduction of area is not reported for tubing or sheet/strip.

Suitability depends on loading, temperature, exposure duration, atmosphere and required service life; no single maximum temperature rating applies. Oxidation resistance is not a substitute for creep or stress-rupture design assessment.

Producer Figures 1–2 show elevated-temperature tensile curves for solution-annealed hot-rolled rod (13 or 16 mm diameter) and cold-rolled sheet (4.75 mm, transverse). Figures 7–8 show creep and rupture curves for solution-annealed bar, tubing and sheet. No numerical tables are transcribed: curve-only data cannot reliably provide exact values and rupture points are not individually tied to product form. Table 7 is exposure/stability data, not an elevated-temperature tensile table. See producer bulletin pages 3, 5–6: https://www.specialmetals.com/documents/technical-bulletins/inconel/inconel-alloy-617.pdf

Solution annealing

Normally used solution annealed. Page 9 specifies 1175 °C for a time commensurate with section size, followed by water quenching or rapid air cooling. Coarse grains support creep-rupture strength and room-temperature bend ductility.

Intermediate annealing for cold forming

Page 9 recommends 1040 °C annealing for cold forming, with fine-grain starting material and frequent intermediate anneals.

Fabricated combustion components

Page 10 discusses mill solution annealing at 1177 °C with water quench, followed by cold forming, welding and re-solution annealing at 1121 °C with air cooling. This application-specific route balances residual cold work and grain coarsening; it is not a universal requirement.

Follow the ordered specification and a qualified procedure. Pages 9 and 10 round the same 2150 °F solution temperature differently (1175 and 1177 °C). No universal hold time or precipitation-ageing schedule is prescribed here.

Material selection

Corrosion resistance & performance

Chromium and nickel support resistance to a range of oxidising and reducing media, but performance is environment-specific. The bulletin does not establish universal aqueous-corrosion immunity.

Producer Table 9 reports 10 g/m² weight gain after 25 h in hydrogen/2% methane at 1095 °C; Table 10 reports 35 g/m² after 100 h in that gas at 980 °C. These carburisation tests are not oxidation ratings or predictions of service life.

Assess actual gas chemistry, contaminants, cycling and surface condition. Chloride and sulphidation resistance in a particular duty must be verified separately; no blanket seawater or sulphur-service approval is implied.

Typical applications

Engineering applications

  • Aircraft and land-based gas-turbine ducting, combustion cans and transition liners
  • Heat-treatment baskets and industrial furnace components
  • Catalyst-grid supports in nitric-acid production
  • Reduction boats for molybdenum refining
  • Selected fossil-fuel and nuclear power-generation components, subject to current code qualification
  • High-temperature heat-exchanger components, subject to engineering assessment and supplier confirmation

Subsequent manufacturing

Machining & processing

Machinability and work hardening

High strength and a high work-hardening rate require a stable setup. Avoid rubbing and repeated dwell; producer guidance calls for sufficient feed and depth to avoid burnishing.

Tooling

Use sharp tools with positive rake angles as recommended by the producer. Select tool grade, coolant and cutting parameters for the actual form, rigidity and condition; no universal cutting speed is stated.

Hot and cold forming

Heavy forming/forging range is 1010–1205 °C; light working may extend down to 925 °C. Cold forming benefits from fine grains and intermediate anneals. Residual cold work can impair subsequent high-temperature creep performance.

Welding

Producer recommends INCONEL Filler Metal 617 for GTAW/GMAW and Welding Electrode 117 for SMAW. Use a qualified procedure and verify filler, joint design and inspection against the duty; filler specifications do not certify the parent metal.

Distortion and heat treatment

Plan fixturing, machining allowances and cooling around section size and geometry. Check dimensional change after forming, welding and heat treatment; the fabrication-specific re-solution route is not an automatic requirement for every part.

Surface finishing

Agree surface finish and scale-removal requirements before ordering. Use controlled finishing and cleaning that avoid embedded contamination and surface damage; validate the process for the application.

Inspection

Agree dimensional, surface and applicable volumetric examinations, acceptance criteria and traceability at enquiry. Verify ordered condition and test orientation; PMI alone does not demonstrate full chemistry, mechanical properties or heat-treatment compliance.

Material certification & testing

Certification and inspection options are subject to customer requirements and supplier confirmation.

Conformity must be demonstrated against the ordered specification, product form and condition. Tests and certificates are not included automatically; agree scope and acceptance criteria before order.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

Inconel 617 Nickel Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.