Stack of pickled Inconel 625 nickel alloy plates of different thicknesses

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

Inconel 625 Nickel Alloy

Solid-solution-strengthened nickel-chromium-molybdenum-niobium alloy | UNS N06625 | W.Nr. 2.4856

Inconel 625 is a nickel-chromium-molybdenum-niobium alloy. Molybdenum and niobium stiffen its nickel-chromium matrix through solid-solution strengthening; precipitation-hardening treatments are not required to obtain its basic strength. Conventional alloy 625 is not 625LCF or another modified grade.

The combination of strength, fabricability and resistance to pitting, crevice attack and chloride stress-corrosion cracking makes it a candidate for demanding aqueous and elevated-temperature equipment. Selection still requires assessment of the actual environment, loading, fabrication and material condition.

INCONEL® is a trademark of the Special Metals Corporation group of companies, as stated in its alloy bulletin. Quest Engineering does not own this trademark.

Raw & semi-finished materials

Available material forms

Bulletin-listed mill forms only. Availability depends on specification, dimensions, condition and supplier confirmation; no stock holding is implied.

  • Rod and Bar
  • Wire and Wire Rod
  • Plate
  • Sheet
  • Strip
  • Shapes
  • Pipe and Tube
  • Forging Stock
  • Cut-to-Size Material

Material overview

Inconel 625 Nickel Alloy

A strong, readily fabricated nickel alloy combining chloride corrosion resistance with useful elevated-temperature properties for qualified marine, chemical and aerospace duties.

  • Solid-solution strengthening without a required precipitation-ageing cycle.
  • Annealed and solution-treated properties differ; product form and section size must accompany any property requirement.
  • Solution-treated material is recommended by the producer when optimum creep or rupture resistance is required; oxidation resistance alone is not a load-bearing design criterion.

Material specifications & designations

Material specifications & designations
Designation / specificationProduct form / scopeNotes
UNS N06625Alloy designationConventional alloy 625; not a product specification.
W.Nr. 2.4856European material numberProducer designation; not proof of compliance with every EN product standard.
EN 10095Rod, bar, sections, plate, sheet and stripProducer-listed; current complete EN scope and grade requirements not independently verified.
ASTM B443Rolled plate, sheet and stripPublic ASTM abstract: N06625 Grade 1 annealed / Grade 2 solution annealed.
ASTM B446Rod and barPublic ASTM scope covers hot- and cold-worked rod and bar; condition and grade must be ordered.
ASTM B444Cold-worked seamless pipe and tubePublic ASTM abstract: N06625 Grade 1 annealed / Grade 2 solution annealed.
ASTM B564Nickel-alloy forgingsPublic historical ASTM scope includes N06625; not a bar standard.
ASTM B704Welded tubeProducer-listed; use with general requirements B751.
ASTM B751General requirements for welded nickel and nickel-alloy tubeCompanion requirements, not an independent alloy purchase specification.
ASTM B705Welded pipeProducer-listed; use with general requirements B775.
ASTM B775General requirements for welded nickel and nickel-alloy pipeCompanion requirements, not an independent alloy purchase specification.
ASTM B829General requirements for seamless nickel and nickel-alloy pipe and tubeProducer-listed companion to B444.
ASTM B366Factory-made wrought nickel-alloy fittingsProducer-listed fittings specification, not tube or bar.
AMS 5666Annealed bars, forgings, extrusions, rings and stock for forging, extrusion and ringsProducer listing and public catalogue scope; finished-product size limits depend on revision.
AMS 5599Annealed sheet, strip and plateSAE public abstract/title verified; not AMS 5869 condition.
AMS 5869Solution-heat-treated sheet, strip and plateSAE public abstract/title verified; not interchangeable with annealed AMS 5599.
AMS 5581Annealed seamless or welded tubingProducer-listed; public catalogue title supports form and condition.

Producer bulletin p.18 associations, supplemented by public abstracts/catalogue titles. Full current ASTM, AMS and EN standards were not accessible for complete compliance verification; confirm revision, grade, dimensions, condition and tests at order. AMS 5837 is welding wire (filler), not parent-metal wire; it is deliberately excluded from parent-metal specifications. No blanket aerospace, NACE or pressure-code approval is implied. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • Designations / ordered product condition

    Six nominal ranges are product-form dependent, not guaranteed acceptance limits; current AMS/ASTM condition and size requirements need controlled verification. Existing cautions do not prove conformity; no allegation that every listed scope is wrong. Obtain the ordered revision and map each cited specification to form, dimensions, manufacture, delivery condition and acceptance tests.

    Obtain licensed ordered editions and issue a material-specific form/condition/size compliance matrix; retain existing caveats pending approval.

Engineering reference

Technical data

Chemical composition
ElementMass %
Nickel58.0 min.
Chromium20.0–23.0
Iron5.0 max.
Molybdenum8.0–10.0
Niobium + tantalum3.15–4.15
Carbon0.10 max.
Manganese0.50 max.
Silicon0.50 max.
Phosphorus0.015 max.
Sulfur0.015 max.
Aluminium0.40 max.
Titanium0.40 max.
Cobalt1.0 max. (if determined)

Single-source limiting chemistry: producer Table 1, p.1. Mass percentages, not a blend of standard limits; Nb + Ta remains combined.

Typical physical properties
PropertyValueTemperature / basis
Density8440 kg/m³Table 2; temperature not specified
Melting range1290–1350 °CTable 2
Specific heat410 J/(kg·K)21 °C; calculated
Specific heat565 J/(kg·K)649 °C; calculated
Electrical resistivity1.29 µΩ·m21 °C
Electrical resistivity1.38 µΩ·m649 °C
Thermal conductivity9.8 W/(m·K)21 °C
Thermal conductivity19.0 W/(m·K)649 °C
Mean linear expansion coefficient12.8 × 10⁻⁶ K⁻¹21–93 °C
Mean linear expansion coefficient14.8 × 10⁻⁶ K⁻¹21–649 °C
Dynamic tensile modulus — annealed207.5 GPa21 °C
Dynamic tensile modulus — solution-treated204.8 GPa21 °C
Dynamic tensile modulus — annealed170.3 GPa649 °C
Dynamic tensile modulus — solution-treated166.5 GPa649 °C

Producer Tables 2–4, pp.2–3; typical, not specification limits. Conductivity/resistivity specimens annealed at 2100 °F for 1 h; modulus dynamically measured on samples from 3/4-in. (19.05 mm) hot-rolled rod. SI density and resistivity converted from 8.44 g/cm³ and µΩ·cm. CTE is mean from 70 °F (approximately 21 °C), not instantaneous.

As-rolled — rod, bar and plate

Room-temperature mechanical properties — As-rolled — rod, bar and plate
PropertyValueBasis
Ultimate tensile strength827–1103 MPaNominal producer range
0.2% offset yield strength414–758 MPaNominal producer range
Elongation30–60%Nominal producer range; gauge length not stated
Hardness175–240 HBBrinell; method details not stated
Reduction of area40–60%Nominal producer range

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Annealed — rod, bar and plate

Room-temperature mechanical properties — Annealed — rod, bar and plate
PropertyValueBasis
Ultimate tensile strength827–1034 MPaNominal producer range
0.2% offset yield strength414–655 MPaNominal producer range
Elongation30–60%Nominal producer range; gauge length not stated
Hardness145–220 HBBrinell; method details not stated
Reduction of area40–60%Nominal producer range

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Solution-treated — rod, bar and plate

Room-temperature mechanical properties — Solution-treated — rod, bar and plate
PropertyValueBasis
Ultimate tensile strength724–896 MPaNominal producer range
0.2% offset yield strength290–414 MPaNominal producer range
Elongation40–65%Nominal producer range; gauge length not stated
Hardness116–194 HBBrinell; method details not stated
Reduction of area60–90%Nominal producer range

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Annealed — sheet and strip

Room-temperature mechanical properties — Annealed — sheet and strip
PropertyValueBasis
Ultimate tensile strength827–1034 MPaNominal producer range
0.2% offset yield strength414–621 MPaNominal producer range
Elongation30–55%Nominal producer range; gauge length not stated
Hardness145–240 HBBrinell; method details not stated

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Annealed — cold-drawn tube and pipe

Room-temperature mechanical properties — Annealed — cold-drawn tube and pipe
PropertyValueBasis
Ultimate tensile strength827–965 MPaNominal producer range
0.2% offset yield strength414–517 MPaNominal producer range
Elongation30–55%Nominal producer range; gauge length not stated
HardnessNot reportedNo value in this Table 5 row

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Solution-treated — cold-drawn tube and pipe

Room-temperature mechanical properties — Solution-treated — cold-drawn tube and pipe
PropertyValueBasis
Ultimate tensile strength689–827 MPaNominal producer range
0.2% offset yield strength276–414 MPaNominal producer range
Elongation40–60%Nominal producer range; gauge length not stated
HardnessNot reportedNo value in this Table 5 row

Producer Table 5, p.3: composites for various product sizes up to 4 in. (101.6 mm); not specification minima or acceptance limits. Ranges displayed low-to-high where the source prints descending elongation/area ranges. Exact specimen geometry, orientation and heat-treatment cycle are not given; consult producer for larger sections. Do not transfer values between forms or conditions.

Suitability depends on loading, temperature, exposure duration, atmosphere and required service life; no single maximum temperature rating applies. Short-time tensile properties, creep resistance and oxidation behaviour are different selection criteria.

Elevated-temperature tensile — hot-rolled annealed bar after 2000 h exposure at each test temperature

Elevated-temperature tensile — hot-rolled annealed bar after 2000 h exposure at each test temperature
Temperature °CUTS MPaYield MPaElongation %
6491010.1734.354
760584.7544.762
871284.1275.880

Producer Table 6, p.4, properties measured at exposure temperature after 2000 h; 0.2% offset yield. Composite product sizes up to 4 in. (101.6 mm); specimen geometry/orientation unspecified. Typical test results, not unexposed tensile data, design allowables or stress-rupture tests.

Figures 11–14 show typical creep/rupture curves for solution-treated and annealed material. Numerical stress-rupture rows are omitted because the curve captions do not establish product form/section/specimen basis and exact tabulated values are unavailable. Obtain qualified form-specific creep data for design. Figure 15 shows cyclic scaling at 1800 °F, but the atmosphere is not specified; no quantitative oxidation claim or universal service limit is inferred.

Annealing

Producer batch guidance: hot- or cold-formed parts are usually annealed at 1700–1900 °F (approximately 927–1038 °C), for times commensurate with thickness. Higher temperatures may be used to soften material for additional cold work.

Solution treatment

Producer batch metal-temperature range: 2000–2200 °F (approximately 1093–1204 °C). Select the ordered specification cycle rather than substituting an anneal or an alloy 718 ageing schedule.

Stress relief

Heating cold-drawn material at 1100–1400 °F (approximately 593–760 °C) reduces residual stress; the bulletin reports virtually complete stress relief at 1600 °F (approximately 871 °C). This is guidance, not a complete qualified time/temperature cycle.

Source p.10. These are metal temperatures for batch operations, not furnace setpoints for continuous annealing. Holding time must reflect thickness and specification. The bulletin states cooling rate has no significant effect in this context; this is not permission to disregard ordered cooling requirements. Intermediate-temperature exposure can harden alloy 625 and alter ductility. No precipitation-ageing schedule is prescribed here.

Material selection

Corrosion resistance & performance

Producer p.10 describes resistance across many oxidising and non-oxidising aqueous environments. Chromium and nickel support oxidising-media resistance; molybdenum and nickel contribute in non-oxidising media. Acid concentration, contaminants and temperature must be checked for each duty.

High molybdenum content supports resistance to chloride pitting and crevice corrosion; high nickel content supports chloride stress-corrosion cracking resistance. Marine use does not imply immunity under every deposit, crevice, stagnant condition or temperature.

Niobium stabilisation supports resistance to weld sensitisation and subsequent intergranular attack. Surface condition, thermal history and qualified welding procedures remain important; the bulletin is not a corrosion allowance or sour-service approval.

Typical applications

Engineering applications

  • Aircraft ducting, engine exhaust and thrust-reverser components
  • Marine fasteners, cable sheathing and oceanographic components
  • Chemical-processing vessels, transfer piping, heat exchangers and valves
  • Bellows, seals and expansion-joint components subject to fatigue design
  • Corrosion-resistant mechanical components for oil and gas equipment, subject to project-specific qualification

Subsequent manufacturing

Machining & processing

Machinability and work hardening

Strength and work hardening make alloy 625 demanding to machine. Plan stable engagement and avoid rubbing or dwelling on a work-hardened surface; qualify parameters for the actual condition and section.

Tooling and cooling

Use rigid workholding, sharp suitable tooling and effective coolant/chip control. Producer Table 12 distinguishes high-speed-steel and coated-carbide turning; it is not a universal speed recommendation for drilling, milling or other operations.

Welding

The producer describes conventional welding processes with Filler Metal 625 or Welding Electrode 112. These are consumables, not parent-metal specifications. Qualify filler selection, joint preparation, cleanliness, heat input and interpass control for the service; do not assume a generic postweld cycle.

Forming

Hot and cold forming are possible, but high deformation resistance requires adequately powerful equipment. Cold working raises strength and hardness and changes ductility; intermediate annealing and springback must be considered. Follow producer hot-working guidance rather than extrapolating room-temperature formability.

Distortion control

Plan balanced machining allowances and welding sequences, suitable fixturing and any specified stress relief. Residual stress removal and thermal exposure can change final dimensions; verify critical tolerances after processing.

Finishing and contamination control

Heat produces adherent oxide unless protected appropriately. The producer discusses fused-salt pretreatment before pickling; use a qualified cleaning/descaling route with appropriate chemical controls. Prevent embedded iron and shop contamination and verify the specified final surface condition.

Inspection

Agree dimensional, surface, weld and volumetric inspection acceptance criteria before supply. PMI supports alloy identification but does not establish heat treatment, all chemical limits or mechanical performance. NDT suitability depends on form, size and ordered specification.

Material certification & testing

Documentation and inspection options are agreed at enquiry for the selected product form and condition.

Conformity must be demonstrated against the ordered specification, revision, form and condition. Tests and certification options are not automatic; agree scope, sampling, acceptance criteria and traceability before order.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

Inconel 625 Nickel Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.