Representative ground nickel-based alloy round bars

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

René 41 Nickel Superalloy

Precipitation-hardening nickel superalloy | UNS N07041

René 41 is a precipitation-hardenable nickel-chromium-cobalt-molybdenum superalloy with aluminium and titanium additions for high-strength elevated-temperature applications.

Turbine and aerospace applications require product-form-specific solution treatment and ageing. Tensile and stress-rupture tables retain their actual treatment bases; typical results are not design allowables.

UDIMET® is a registered trademark of Special Metals Corporation. Producer literature also describes R41; Quest Engineering does not claim ownership of proprietary alloy names or manufacture the alloy.

Raw & semi-finished materials

Available material forms

Producer-supported product forms; availability is subject to ordered specification, dimensions and supplier confirmation. No Quest Engineering stockholding is implied.

  • Forging billet
  • Bar
  • Sheet
  • Plate

Material overview

René 41 Nickel Superalloy

Age-hardenable nickel superalloy for highly stressed gas-turbine components.

  • Nickel-chromium-cobalt-molybdenum alloy strengthened by aluminium- and titanium-bearing gamma-prime precipitates.
  • The archived Haynes sheet tensile table retains its own solution, re-treatment and ageing sequence; it does not establish properties for the separate Carpenter bar schedules.
  • Full ordered standards, residual chemistry limits and condition-specific bar testing require confirmation.

Specifications and designations

Specifications and designations
ReferenceProducer-listed scope / status
UNSN07041
AMS5545; AMS5712; AMS5713Producer major specifications; forms available: forging billet, bar, sheet and plate; no one-to-one scope mapping verified

No full standards reviewed. SAE direct public scope retrieval unsuccessful. Confirm edition, product scope and condition before ordering. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • Specifications / product form

    Producer listings and historic references support alloy association but not every listed standard’s current revision, individual form, section-size, melt-route, heat-treatment tolerances or acceptance requirements. Existing qualification wording is appropriate, not proof of conformity.

    Obtain controlled ordered-standard and producer confirmation before technical release.

  • Mechanical condition selectors

    Explicit unavailable/not-verified values are correctly distinguished from zero, but selected conditions cannot support a numeric purchasing comparison. Do not fill aged conditions from annealed tables or graph estimates.

    Obtain form-, section-, orientation-, temperature- and condition-matched producer or specification tables; otherwise retain explicit gaps.

Engineering reference

Technical data

Chemical composition
ElementMinimum mass %Maximum mass %
C0.060.12
Mn—0.10
Si—0.20
Cr18.0020.00
NiBalanceBalance
Mo9.0010.50
Co10.0012.00
Ti3.003.30
Al1.401.60
B0.0030.010
Fe—5.00

Complete single-source producer Type Analysis table, mass %. Single figures nominal except where noted; maxima and ranges reproduced. Sulfur, phosphorus, copper and other unlisted residual limits are not supplied by this source and are not inferred. Carpenter Al and C limits differ from Special Metals; sources are not merged.

Physical constants
PropertyValueUnitTemperature / interval
Density8250kg/m³Not stated
Melting range1232–1391°CRange
Specific heat435J/(kg·K)Not stated
Thermal conductivity9.0W/(m·K)Not stated
Mean thermal expansion11.910⁻⁶/K21–93°C

Temperatures not stated must not be silently labelled room temperature. Carpenter converted SI series are retained separately in research JSON.

Sheet — 1079°C solution treated, 1066°C re-treated and aged

Room-temperature mechanical properties — Sheet — 1079°C solution treated, 1066°C re-treated and aged
PropertyTypical valueBasis
Ultimate tensile strength1343 MPa (194,800 psi)21°C (70°F)
0.2% yield strength1070 MPa (155,200 psi)21°C (70°F)
Elongation14%2 in (50.8 mm) gauge length
HardnessNot tabulated for this conditionDo not substitute hardness from a different treatment
Proportional limit807 MPa (117,100 psi)21°C (70°F)
Elastic modulus222 GPa (32.2 × 10⁶ psi)21°C (70°F)
Reduction of areaNot tabulatedNo condition-matched value verified

Sheet 0.050 in (1.27 mm); 1975°F (1079°C) solution heat treated, water quenched (initial hold not stated), then 1950°F (1066°C) / 30 min AC, then 1400°F (760°C) / 16 h AC. Strain rate 0.005 in/in/min through a point beyond 0.2% yield. Typical/average laboratory values, not minima. psi × 0.006894757293 = MPa. Archived Haynes-authored document; current official host remained blocked. Typical producer values, not specification minima or design allowables; confirm ordered condition, section limits, specimen requirements and gauge length where not stated.

Bar — fine-grain solution treated and aged

Mechanical properties — 1038–1052°C / 4 h AC + 760°C / 16 h AC
PropertyValue / statusBasis
Ultimate tensile strengthNot verifiedNo numerical condition-matched producer table accessed
0.2% proof / yield strengthNot verifiedNo graph-derived values
ElongationNot verifiedNo numerical condition-matched producer table accessed
HardnessNot tabulated for this exact conditionGeneral ageing hardness is not a condition-specific result
Reduction of areaNot tabulatedNo condition-matched value verified

Room-temperature tensile table unavailable; hardness is general treatment guidance, not a guaranteed condition-specific acceptance value. Typical producer values, not specification minima or design allowables; confirm ordered condition, section limits, specimen requirements and gauge length where not stated.

Bar — rupture-oriented solution treated and aged

Mechanical properties — 1080°C / 1 h AC + 760°C / 16 h AC
PropertyValue / statusBasis
Ultimate tensile strengthNot verifiedNo numerical condition-matched producer table accessed
0.2% proof / yield strengthNot verifiedNo graph-derived values
ElongationNot verifiedNo numerical condition-matched producer table accessed
HardnessNot tabulated for this exact conditionGeneral ageing hardness is not a condition-specific result
Reduction of areaNot tabulatedNo condition-matched value verified

Room-temperature tensile table unavailable; hardness is general treatment guidance, not a guaranteed condition-specific acceptance value. Typical producer values, not specification minima or design allowables; confirm ordered condition, section limits, specimen requirements and gauge length where not stated.

Precipitation-hardened UDIMET R41 rupture data; exact cycle and product unspecified.

Table 3 1000-hour rupture strength

Table 3 1000-hour rupture strength
Test temperature (°C)Rupture stress (MPa)
649705
704550
760345
816200
871117
92776

Precipitation hardened; exact cycle and product not specified

Condition-specific tensile data — 1.27 mm sheet

Condition-specific tensile data — 1.27 mm sheet
Test temperature (°C)Test temperature (°F)UTS (MPa)0.2% yield strength (MPa)Elongation in 50.8 mm (%)Proportional limit (MPa)Elastic modulus (GPa)
21.1701343.11070.114807.4222.0
537.810001187.3969.414702.6165.5
648.912001179.0930.18666.7162.0
760.014001041.8862.56666.7133.1
871.11600733.6562.65355.8120.0
982.21800286.1176.515121.3111.7
1093.3200078.639.34730.3Not tabulated

Sheet 0.050 in (1.27 mm); 1975°F (1079°C) solution heat treated, water quenched (initial hold not stated), then 1950°F (1066°C) / 30 min AC, then 1400°F (760°C) / 16 h AC. Strain rate 0.005 in/in/min through a point beyond 0.2% yield. Typical/average laboratory values, not minima. psi × 0.006894757293 = MPa. Archived Haynes-authored document; current official host remained blocked.

Oxidation performance

  • Carpenter describes resistance to jet-engine combustion gases up to 982°C; no quantitative mass-change/penetration table verified.

1000-hour rupture strengths are not tensile values. No graph reading. Separate archived Haynes sheet tensile table added; do not assign its values to Carpenter schedules. Suitability depends on loading, temperature, atmosphere, exposure duration and required service life. Test temperatures are not universal maximum service temperatures.

Fine grain and best tensile ductility

1038-1052 C 4h air cool → 760 C 16h air cool [CT p4] Source: https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/Pyromet%2041.pdf

Improved stress rupture

1080 C 1h air cool → 760 C 16h air cool [CT p4] Source: https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/Pyromet%2041.pdf

Low-hardness anneal

1066 C quench [CT p4] Source: https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/Pyromet%2041.pdf

Sheet — 1079°C solution treated, 1066°C re-treated and aged

Sheet 0.050 in (1.27 mm); 1975°F (1079°C) solution heat treated, water quenched (initial hold not stated), then 1950°F (1066°C) / 30 min AC, then 1400°F (760°C) / 16 h AC. Strain rate 0.005 in/in/min through a point beyond 0.2% yield. Typical/average laboratory values, not minima. psi × 0.006894757293 = MPa. Archived Haynes-authored document; current official host remained blocked. Source: https://www.spacematdb.com/spacemat/manudatasheets/r41.pdf

Independent producer schedules; do not splice or treat alternatives as universally qualified. Carpenter p4; high-temperature carbide solutioning can impair ductility.

Material selection

Corrosion resistance & performance

Oxidation resistance does not establish resistance to all hot-corrosion or aqueous environments. Confirm atmosphere, temperature and stress for the intended application.

Typical applications

Engineering applications

  • afterburner parts
  • turbine casings
  • wheels and buckets
  • bolts and fasteners
  • nozzle partitions
  • combustion chamber liners

Subsequent manufacturing

Machining & processing

Processing precautions

Rapid work hardening, frequent anneals; Avoid small cold sizing reductions; strain-age cracking risk; Heat cold-worked sections rapidly through 649-927 C to solution/anneal temperature; Above 1149 C carbide solution can cause continuous grain boundary M23C6 and low ductility

Machining condition and tooling

Confirm the actual material condition before planning machining. Allow for work hardening; qualify tool material, rigidity, coolant and cutting engagement for the product. No universal speeds or feeds are specified.

Distortion, finishing and inspection

Agree machining allowance, final surface condition and dimensional inspection around heat treatment. Define surface and internal inspection, acceptance criteria and traceability to the ordered specification; additional testing is not automatic.

Material certification & testing

Certification and inspection options are subject to customer requirements and supplier confirmation.

Conformity must be demonstrated against the ordered specification, form and condition. Tests are not automatic; agree scope, acceptance criteria and documentation before ordering.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

René 41 Nickel Superalloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.