Materials Supply / Nickel, Cobalt & High-Temperature Alloys
Nimonic 105 Nickel Alloy
Age-hardenable wrought nickel-cobalt-chromium alloy | W.Nr. 2.4634
Nimonic 105 is a precipitation-hardenable nickel-cobalt-chromium alloy containing molybdenum, aluminium and titanium. It was developed for high-strength elevated-temperature applications, with distinct treatment routes for long-term creep performance and tensile-led fastener applications.
NIMONIC® alloy 105 for high-temperature components, with properties dependent on product form and heat treatment.
NIMONIC® is a trademark of the Special Metals Corporation group of companies. Quest Engineering supplies materials to customer requirements and does not manufacture or own this alloy trademark.
Raw & semi-finished materials
Available material forms
Producer-supported forms; availability, dimensions and ordered specification require supplier confirmation. No Quest stockholding is implied.
- Round bar
- Flat bar
- Forging stock
- Extruded section
- Billet
- Rod
- Extruded and cold-worked section
Material overview
Nimonic 105 Nickel Alloy
NIMONIC® alloy 105 for high-temperature components, with properties dependent on product form and heat treatment.
- Select the actual processing condition when comparing mechanical properties. Producer data are typical or average results, not guaranteed minima or design allowables.
- Historical specification references require full-standard review before procurement.
Material specifications & designations
| Designation / standard | Scope / condition |
|---|---|
| W.Nr. | 2.4634 |
| BS HR3 | Historical reference — Billets, bars and forgings |
| AICMA Ni-P61-HT | Historical reference — Billets, bars and forgings |
| Swedish Defence MH.14 | Historical reference — Forged bar |
| DIN designation | NiCo20Cr15MoAlTi — Forged bar; designation, not numbered standard |
| AFNOR designation | NCKD 20ATv — Form/condition scope not supplied |
| AECMA PrEN2179–2181 | Historical grouped reference — Individual form/condition scope not verified |
Source: bulletin p18 (90) or p23 (105). No full standard acceptance requirements verified. The proposed UNS N09105 could not be verified in an authoritative source and is omitted. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.
Specification review
Technical verification requirements
Specifications / product form
Producer listings and historic references support alloy association but not every listed standard’s current revision, individual form, section-size, melt-route, heat-treatment tolerances or acceptance requirements. Existing qualification wording is appropriate, not proof of conformity.
Obtain controlled ordered-standard and producer confirmation before technical release.
UNS / identity
Accessed SMC-081 identifies 2.4634 but does not establish a UNS. The current omission is appropriately conservative; do not insert N09105 from unsupported secondary listings.
Request authoritative producer/UNS registration confirmation; preserve omission until established.
Engineering reference
Technical data
| Element | Minimum mass % | Maximum mass % |
|---|---|---|
| Carbon | — | 0.17 |
| Silicon | — | 1.0 |
| Copper | — | 0.2 |
| Iron | — | 1.0 |
| Manganese | — | 1.0 |
| Chromium | 14.0 | 15.7 |
| Titanium | 0.9 | 1.5 |
| Aluminium | 4.5 | 4.9 |
| Cobalt | 18.0 | 22.0 |
| Molybdenum | 4.5 | 5.5 |
| Lead | — | 0.0015 |
| Sulphur | — | 0.010 |
| Boron | 0.003 | 0.010 |
| Zirconium | — | 0.15 |
| Nickel | Balance | Balance |
Single primary source: bulletin p1. Nickel balance is not a numeric minimum. Composition expressly stated as BS HR3.
| Property | Value | Unit | Temperature / range |
|---|---|---|---|
| Density | 8010 | kg/m³ | Temperature not explicitly stated |
| Solidus | 1290 | °C | Melting |
| Liquidus | 1345 | °C | Melting |
| Specific heat | 419 | J/(kg·K) | 20°C |
| Thermal conductivity | 10.89 | W/(m·K) | 20°C |
| Mean coefficient of thermal expansion | 12.2 | µm/(m·K) | 20–100°C |
| Electrical resistivity | 1.31 | µΩ·m | 20°C |
| Dynamic Young’s modulus — extruded bar | 188 | GPa | 20°C |
| Dynamic Young’s modulus — subsequently forged | 223 | GPa | 20°C |
| Dynamic Young’s modulus — subsequently cold rolled | 220 | GPa | 20°C |
Bulletin physical-property tables. Moduli are condition-specific, not universal static design constants. Full test-conditioning notes and temperature arrays are in the research file. Density temperature is not supplied.
Extruded bar — three-stage treatment A
| Property | Typical value | Unit |
|---|---|---|
| Tensile strength | 1140 | MPa |
| 0.1% proof stress | 751 | MPa |
| 0.2% proof stress | 776 | MPa |
| Elongation | 22 | % |
| Reduction of area | 31 | % |
Table 7; 20°C. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Elongation gauge: 5.65√S0. Average/typical results, not acceptance minima. Hardness not tabulated.
Extruded bar subsequently forged — three-stage treatment A
| Property | Typical value | Unit |
|---|---|---|
| Tensile strength | 1180 | MPa |
| 0.1% proof stress | 796 | MPa |
| 0.2% proof stress | 827 | MPa |
| Elongation | 16 | % |
| Reduction of area | 16 | % |
Table 8; 20°C. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Elongation gauge: 5.65√S0. Average/typical results, not acceptance minima. Hardness not tabulated.
Extruded section subsequently cold rolled — three-stage treatment A
| Property | Typical value | Unit |
|---|---|---|
| Tensile strength | 1246 | MPa |
| 0.1% proof stress | 795 | MPa |
| 0.2% proof stress | 826 | MPa |
| Elongation | 25 | % |
| Reduction of area | 29 | % |
Table 9; 20°C. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Elongation gauge: 5.55√S0 (printed source value). Average/typical results, not acceptance minima. Hardness not tabulated.
Extruded bar subsequently cold stretched — two-stage treatment B
| Property | Typical value | Unit |
|---|---|---|
| Tensile strength | 1220 | MPa |
| 0.1% proof stress | 791 | MPa |
| 0.2% proof stress | 811 | MPa |
| Elongation | 25 | % |
| Reduction of area | 35 | % |
Table 10; 20°C. 4 h at 1125°C, air cool; 16 h at 850°C, air cool. Elongation gauge: 5.55√S0 (printed source value). Average/typical results, not acceptance minima. Hardness not tabulated.
Tabulated producer data only. Preserve form and heat treatment when comparing values.
Extruded bar — three-stage treatment A — elevated-temperature tensile
| Temperature (°C) | UTS (MPa) | 0.1% proof (MPa) | 0.2% proof (MPa) | Elongation (%) | Reduction of area (%) |
|---|---|---|---|---|---|
| 100 | 1123 | 739 | 762 | 20 | 31 |
| 200 | 1084 | 712 | 735 | 21 | 38 |
| 300 | 1091 | 712 | 735 | 20 | 30 |
| 400 | 1101 | 718 | 743 | 24 | 39 |
| 500 | 1064 | 711 | 740 | 23 | 37 |
| 600 | 1038 | 694 | 720 | 25 | 38 |
| 700 | 1018 | 706 | 732 | 28 | 36 |
| 800 | 813 | 647 | 677 | 25 | 37 |
| 900 | 496 | 373 | 400 | 30 | 47 |
| 1000 | 175 | 144 | 152 | 42 | 73 |
| 1100 | 51 | 26 | 29 | 172 | 99 |
Table 7. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.
Extruded bar subsequently forged — three-stage treatment A — elevated-temperature tensile
| Temperature (°C) | UTS (MPa) | 0.1% proof (MPa) | 0.2% proof (MPa) | Elongation (%) | Reduction of area (%) |
|---|---|---|---|---|---|
| 100 | 1185 | 760 | 793 | 21 | 24 |
| 200 | 1188 | 745 | 774 | 24 | 34 |
| 300 | 1162 | 739 | 766 | 20 | 24 |
| 400 | 1126 | 732 | 763 | 23 | 33 |
| 500 | 1148 | 748 | 782 | 23 | 31 |
| 600 | 1111 | 735 | 769 | 22 | 32 |
| 700 | 1075 | 739 | 768 | 26 | 33 |
| 800 | 836 | 680 | 714 | 24 | 34 |
| 900 | 491 | 390 | 411 | 28 | 38 |
| 1000 | 189 | 152 | 156 | 43 | 60 |
| 1100 | 56 | 28 | 31 | 132 | 99 |
Table 8. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.
Extruded section subsequently cold rolled — three-stage treatment A — elevated-temperature tensile
| Temperature (°C) | UTS (MPa) | 0.1% proof (MPa) | 0.2% proof (MPa) | Elongation (%) | Reduction of area (%) |
|---|---|---|---|---|---|
| 100 | 1220 | 780 | 811 | 24 | 30 |
| 200 | 1234 | 755 | 785 | 26 | 31 |
| 300 | 1239 | 744 | 772 | 26 | 31 |
| 400 | 1226 | 744 | 783 | 27 | 31 |
| 500 | 1195 | 752 | 785 | 27 | 31 |
| 600 | 1177 | 743 | 775 | 25 | 31 |
| 700 | 1092 | 744 | 778 | 31 | 31 |
| 800 | 856 | 681 | 718 | 25 | 31 |
| 900 | 533 | 392 | 420 | 31 | 39 |
| 1000 | 221 | 168 | 176 | 48 | 61 |
Table 9. 4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.
Extruded bar subsequently cold stretched — two-stage treatment B — elevated-temperature tensile
| Temperature (°C) | UTS (MPa) | 0.1% proof (MPa) | 0.2% proof (MPa) | Elongation (%) | Reduction of area (%) |
|---|---|---|---|---|---|
| 100 | 1177 | 749 | 777 | 24 | 39 |
| 200 | 1186 | 731 | 757 | 27 | 34 |
| 300 | 1183 | 732 | 752 | 25 | 36 |
| 400 | 1143 | 740 | 760 | 28 | 35 |
| 500 | 1140 | 740 | 771 | 28 | 35 |
| 600 | 1106 | 726 | 759 | 26 | 35 |
| 700 | 1060 | 723 | 752 | 30 | 33 |
| 800 | 817 | 678 | 706 | 27 | 35 |
| 900 | 496 | 407 | 430 | 27 | 35 |
Table 10. 4 h at 1125°C, air cool; 16 h at 850°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.
Continuous air oxidation — 100 h
| Temperature (°C) | Descaled weight loss (mg/cm²) |
|---|---|
| 800 | 0.11 |
| 900 | 0.49 |
| 950 | 0.99 |
| 1000 | 1.43 |
| 1100 | 6.41 |
Producer p. 22. Exposure test, not service-temperature qualification. Representative producer data; not guaranteed specification limits.
Oxidation performance
- See the 100 h continuous-air test table. Intermittent and cyclic data are distinct tests and must not be combined.
No graph estimates. Creep-rupture analysis tables, including source extrapolation flags, are retained in the technical review notes, not promoted here to guaranteed properties. Extruded-bar stress relaxation is not spring-wire qualification. Suitability depends on stress, temperature, exposure duration, atmosphere and required service life; test temperatures are not universal service ratings.
Treatment A — creep route
4 h at 1150°C, air cool; 16 h at 1050–1065°C, air cool; 16 h at 850°C, air cool. Intended for optimum long-term creep strength and ductility at 850–950°C; blades, discs, forgings and rings.
Treatment B — fastener route
4 h at 1125°C, air cool; 16 h at 850°C, air cool. Extruded/cold-worked stock for bolts and fasteners; cooling from 1125°C must be free and not delayed by packing.
Interstage anneal
1150°C followed by air cooling or fluidized-bed quenching. No duration stated. Water quenching is not recommended: severe surface cracking may result.
Do not apply NIMONIC 90 ageing schedules to alloy 105. Treatment B is not an equivalent long-term creep qualification.
Material selection
Corrosion resistance & performance
Oxidation performance depends on exposure cycle, atmosphere, time and temperature; no unconditional operating-temperature rating is implied.
Typical applications
Engineering applications
- Turbine blades
- Turbine discs
- Forgings
- Ring sections
- Bolts and fasteners
Subsequent manufacturing
Machining & processing
Hot working
1050–1200°C.
Machining
Machine fully heat treated. Producer prose hardness range 320–385 HV; tungsten-carbide tipped tools recommended. This is not a condition-specific tabulated hardness guarantee.
Welding
Conventional TIG/MIG not recommended due to microfissuring. Electron-beam welding requires trials; flash-butt welding is used for turbine rings.
Material certification & testing
Certification and inspection options are subject to customer requirements and supplier confirmation.
Conformity must be demonstrated against the ordered specification, form and condition. Tests are not automatic; agree scope, acceptance criteria and documentation before ordering.
- EN 10204 3.1 material certificates
- Certificates of Conformity
- Heat/batch traceability
- Chemical analysis
- Mechanical testing
- Heat-treatment records
- Hardness testing
- Positive Material Identification (PMI)
- Ultrasonic testing where applicable
- Additional aerospace or customer-specific inspection requirements
Material enquiry
Request a material quotation
Nimonic 105 Nickel Alloy supplied to your material form, dimensions and specification.