Representative ground nickel-based alloy round bars

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

Nimonic 75 Nickel Alloy

Oxidation-resistant nickel-chromium alloy | UNS N06075 | W.Nr. 2.4951; 2.4630

Nimonic 75 is a nickel-chromium alloy with controlled titanium and carbon additions, used for oxidation and scaling resistance in elevated-temperature sheet and furnace applications. It is principally solid-solution strengthened, not a conventional precipitation-hardening Nimonic grade.

A readily fabricated nickel-chromium alloy for oxidation-resistant sheet and furnace applications.

NIMONIC® is a trademark of the Special Metals Corporation group of companies. Quest Engineering supplies materials to customer requirements and does not manufacture or own this alloy trademark.

Raw & semi-finished materials

Available material forms

Producer-supported forms; availability, dimensions and ordered specification require supplier confirmation. No Quest stockholding is implied.

  • Sheet
  • Strip
  • Plate
  • Round bar
  • Forging stock
  • Wire
  • Tube
  • Extruded section

Material overview

Nimonic 75 Nickel Alloy

A readily fabricated nickel-chromium alloy for oxidation-resistant sheet and furnace applications.

  • Solid-solution nickel-chromium alloy with controlled titanium and carbon additions; not an age-hardening alloy. Annealing must not be described as an ageing treatment.
  • No graph-derived tensile or creep values are included. Unavailable properties are not zero. Werkstoff numbers are listed without an unsupported form-to-number mapping.

Material specifications & designations

Material specifications & designations
Designation / standardScope / condition
UNSN06075
Werkstoff2.4951; 2.4630
BS HR 5; BS HR 504; DIN 17752; AECMA PrEN 2306, 2307, 2402; ISO 9723–25Producer specification references — Rod, bar, wire and forging stock heading; individual scope/condition requires full-standard verification
BS HR 203; DIN 17750; AECMA PrEN 2293, 2302, 2411; ISO 6208Producer specification references — Plate, sheet and strip
BS HR 403; DIN 17751; AECMA PrEN 2294; ISO 6207Producer specification references — Pipe and tube
DIN 17742; AECMA PrEN 2308Producer specification references — Other product forms
AFNOR NC20T; AICMA Ni-P91HT; DIN NiCr20TiOther producer designations — Not independent certification claims

No applicable AMS match was independently verified from SAE. No AMS equivalence is asserted. Specification lists do not establish current editions or supply-condition requirements. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • Specifications / product form

    Producer listings and historic references support alloy association but not every listed standard’s current revision, individual form, section-size, melt-route, heat-treatment tolerances or acceptance requirements. Existing qualification wording is appropriate, not proof of conformity.

    Obtain controlled ordered-standard and producer confirmation before technical release.

  • Mechanical condition selectors

    Explicit unavailable/not-verified values are correctly distinguished from zero, but selected conditions cannot support a numeric purchasing comparison. Do not fill aged conditions from annealed tables or graph estimates.

    Obtain form-, section-, orientation-, temperature- and condition-matched producer or specification tables; otherwise retain explicit gaps.

Engineering reference

Technical data

Chemical composition
ElementMinimum mass %Maximum mass %
Carbon0.080.15
Chromium18.021.0
Copper—0.5
Iron—5.0
Manganese—1.0
Silicon—1.0
Titanium0.20.6
NickelBalanceBalance

Single producer table: as BS HR 203. Balance means nickel predominates; it does not guarantee the entire remainder is nickel. No additional unlisted residual limits are inferred.

Physical properties with temperature and condition basis
PropertyValueSI unitTemperature / interval
Density8370kg/m³Not stated
Melting range1340–1380°CSolidus–liquidus
Specific heat461J/(kg·K)20°C
Thermal conductivity11.7W/(m·K)20°C
Electrical resistivity1.09µΩ·m20°C
Dynamic Young’s modulus221GPa20°C
Dynamic Young’s modulus216GPa100°C
Dynamic Young’s modulus210GPa200°C
Dynamic Young’s modulus203GPa300°C
Dynamic Young’s modulus197GPa400°C
Dynamic Young’s modulus190GPa500°C
Dynamic Young’s modulus181GPa600°C
Dynamic Young’s modulus173GPa700°C
Dynamic Young’s modulus165GPa800°C
Dynamic Young’s modulus153GPa900°C
Dynamic Young’s modulus140GPa1000°C
Mean linear expansion11.010⁻⁶ K⁻¹20–100°C
Mean linear expansion12.710⁻⁶ K⁻¹20–200°C
Mean linear expansion13.410⁻⁶ K⁻¹20–300°C
Mean linear expansion13.910⁻⁶ K⁻¹20–400°C
Mean linear expansion14.310⁻⁶ K⁻¹20–500°C
Mean linear expansion15.010⁻⁶ K⁻¹20–600°C
Mean linear expansion15.410⁻⁶ K⁻¹20–700°C
Mean linear expansion16.510⁻⁶ K⁻¹20–800°C
Mean linear expansion17.110⁻⁶ K⁻¹20–900°C
Mean linear expansion18.210⁻⁶ K⁻¹20–1000°C

Density measurement temperature unspecified. Mean expansion uses 20°C as its lower reference, not negative temperatures. Expansion on fully heat-treated material; approximately ±5% processing variation. Dynamic modulus measured on fully heat-treated cylindrical specimens.

Annealed bar

Annealed bar mechanical properties
PropertyReference valueBasis
Ultimate tensile strengthNot tabulatedGraph-only producer data; no numerical value inferred
0.2% proof strengthNot tabulatedGraph-only producer data; no numerical value inferred
ElongationNot tabulatedGraph-only producer data; no numerical value inferred
HardnessNot tabulatedGraph-only producer data; no numerical value inferred
Reduction of areaNot tabulatedGraph-only producer data; no numerical value inferred

30–60 minutes at 1050°C, air cool. The producer identifies this condition but does not tabulate its tensile values. Obtain specification or supplier data; these blanks are not zero or guaranteed properties.

Annealed sheet

Annealed sheet mechanical properties
PropertyReference valueBasis
Ultimate tensile strengthNot tabulatedGraph-only producer data; no numerical value inferred
0.2% proof strengthNot tabulatedGraph-only producer data; no numerical value inferred
ElongationNot tabulatedGraph-only producer data; no numerical value inferred
HardnessNot tabulatedGraph-only producer data; no numerical value inferred
Reduction of areaNot tabulatedGraph-only producer data; no numerical value inferred

5–10 minutes at 1050°C, air cool. The producer identifies this condition but does not tabulate its tensile values. Obtain specification or supplier data; these blanks are not zero or guaranteed properties.

No elevated-temperature tensile values have been extracted from graphs. No numerical creep table is available in this bulletin.

Oxidation: intermittent heating

Oxidation: intermittent heating
Temperature °CDescaled weight loss after 100 h mg/cm²
9002.25
9504.61
10004.68
110014.1

Cooled to room temperature every 24 hours. Representative producer data; not guaranteed specification limits.

Oxidation performance

  • Oxidation data describe specific laboratory exposures, not a safe working temperature for every load or atmosphere.

Representative producer values only. Suitability depends on stress, temperature, exposure duration, atmosphere and required service life; test temperatures are not universal service ratings.

Bar anneal

30–60 minutes at 1050°C, followed by air cooling.

Sheet anneal

5–10 minutes at 1050°C, followed by air cooling.

Sheet before welding

5–10 minutes at 1050°C / air cool + optional 10 minutes at 1050°C / air cool.

Do not transfer schedules between forms or assume treatment tolerances from these nominal producer recommendations. No ageing stage applies.

Material selection

Corrosion resistance & performance

Oxidation and scaling resistance is an application feature; producer test results are not universal service-temperature guarantees.

No general aqueous-corrosion, NACE or code approval is inferred.

Typical applications

Engineering applications

  • Gas turbine engineering
  • Industrial thermal processing
  • Furnace components
  • Heat-treatment equipment

Subsequent manufacturing

Machining & processing

Hot working

1220–950°C.

Cold working / machining

Annealed material is ductile and readily cold-deformed but strain-hardens rapidly.

Welding

Prefer annealed material. A small amount of cold work may be tolerable. Post-weld heat treatment is normally unnecessary; some chemical service may warrant stress relief. MMA, TIG, MIG, submerged arc, electron beam, oxyacetylene and resistance welding are described.

Material certification & testing

Certification and inspection options are subject to customer requirements and supplier confirmation.

Conformity must be demonstrated against the ordered specification, form and condition. Tests are not automatic; agree scope, acceptance criteria and documentation before ordering.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

Nimonic 75 Nickel Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.