Representative ground nickel-based alloy round bars

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

Nimonic 90 Nickel Alloy

Age-hardenable wrought nickel-cobalt-chromium alloy | UNS N07090 | W.Nr. 2.4632

Nimonic 90 is a wrought precipitation-hardenable nickel-chromium-cobalt alloy strengthened by aluminium and titanium additions, developed for gas-turbine components and demanding elevated-temperature applications.

NIMONIC® alloy 90 for high-temperature components, with properties dependent on product form and heat treatment.

NIMONIC® is a trademark of the Special Metals Corporation group of companies. Quest Engineering supplies materials to customer requirements and does not manufacture or own this alloy trademark.

Raw & semi-finished materials

Available material forms

Producer-supported forms; availability, dimensions and ordered specification require supplier confirmation. No Quest stockholding is implied.

  • Round bar
  • Flat bar
  • Forging stock
  • Extruded section
  • Sheet
  • Strip
  • Plate
  • Wire

Material overview

Nimonic 90 Nickel Alloy

NIMONIC® alloy 90 for high-temperature components, with properties dependent on product form and heat treatment.

  • Select the actual processing condition when comparing mechanical properties. Producer data are typical or average results, not guaranteed minima or design allowables.
  • Historical specification references require full-standard review before procurement.
  • Spring suitability must be evaluated against design stress, temperature, duration and required service life. The reviewed producer bulletin does not provide spring stress-relaxation test conditions or a universal spring temperature rating.

Material specifications & designations

Material specifications & designations
Designation / standardScope / condition
UNSN07090
W.Nr.2.4632
BS HR2 / HR501 / HR502 / HR503Historical grouped references — Rod, bar, wire and forging stock; individual condition/form scope requires full standards
SAE AMS5829Welding wire only; vacuum induction melted — Not structural bar, spring-wire or forging qualification
AECMA PrEN2295 / 2296 / 2297 / 2400 / 2401 / 2669 / 2670Historical grouped references — Rod/bar/wire/forging-stock group; individual scope unverified
BS HR202 / AECMA PrEN2298Historical references — Plate, sheet, strip
BS HR402 / AECMA PrEN2299Historical references — Pipe and tube; availability subject to enquiry

Source: bulletin p18 (90) or p23 (105). No full standard acceptance requirements verified. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • Specifications / product form

    Producer listings and historic references support alloy association but not every listed standard’s current revision, individual form, section-size, melt-route, heat-treatment tolerances or acceptance requirements. Existing qualification wording is appropriate, not proof of conformity.

    Obtain controlled ordered-standard and producer confirmation before technical release.

  • Spring performance

    Spring stress-relaxation evidence remains absent. Tensile tables and recommended sheet/bar ageing are not spring qualification data. This is an evidence gap, not a confirmed erroneous spring claim.

    Obtain spring-wire producer test basis before adding spring performance. Preserve omission.

Engineering reference

Technical data

Chemical composition
ElementMinimum mass %Maximum mass %
Carbon—0.13
Silicon—1.0
Copper—0.2
Iron—1.5
Manganese—1.0
Chromium18.021.0
Titanium2.03.0
Aluminium1.02.0
Cobalt15.021.0
Boron—0.02
Sulphur—0.015
Lead—0.0020
Zirconium—0.15
NickelBalanceBalance

Single primary source: bulletin p1. Nickel balance is not a numeric minimum. Unlisted elements are not asserted to be zero.

SI physical properties
PropertyValueUnitTemperature / range
Density8180kg/m³Temperature not explicitly stated
Solidus1310°CMelting
Liquidus1370°CMelting
Specific heat446J/(kg·K)20°C
Thermal conductivity11.47W/(m·K)20°C
Mean coefficient of thermal expansion12.7µm/(m·K)20–100°C
Electrical resistivity1.18µΩ·m20°C
Dynamic Young’s modulus — extruded bar204GPa20°C
Dynamic Young’s modulus — subsequently forged226GPa20°C
Dynamic Young’s modulus — subsequently cold rolled222GPa20°C

Bulletin physical-property tables. Moduli are condition-specific, not universal static design constants. Full test-conditioning notes and temperature arrays are in the research file. Density temperature is not supplied.

Extruded bar — solution treated and aged

Room-temperature mechanical properties
PropertyTypical valueUnit
Tensile strength1175MPa
0.1% proof stress729MPa
0.2% proof stress752MPa
Elongation30%
Reduction of area47%

Table 8; 20°C. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Elongation gauge: 5.65√S0. Average/typical results, not acceptance minima. Hardness not tabulated.

Extruded bar subsequently forged — solution treated and aged

Room-temperature mechanical properties
PropertyTypical valueUnit
Tensile strength1251MPa
0.1% proof stress791MPa
0.2% proof stress813MPa
Elongation28%
Reduction of area41%

Table 9; 20°C. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Elongation gauge: 5.65√S0. Average/typical results, not acceptance minima. Hardness not tabulated.

Extruded section subsequently cold rolled — solution treated and aged

Room-temperature mechanical properties
PropertyTypical valueUnit
Tensile strength1265MPa
0.1% proof stress813MPa
0.2% proof stress831MPa
Elongation30%
Reduction of area45%

Table 10; 20°C. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Elongation gauge: 5.65√S0. Average/typical results, not acceptance minima. Hardness not tabulated.

Cold-rolled sheet — tested three-stage treatment

Room-temperature mechanical properties
PropertyTypical valueUnit
Tensile strength1180MPa
0.1% proof stress808MPa
0.2% proof stress831MPa
Elongation23%

Table 11; 20°C. 2–3 min at 1150°C, fluidized-bed quench; 20 min at 1040°C, air cool; 4 h at 750°C, air cool. Elongation gauge: 50 mm. Average/typical results, not acceptance minima. Hardness not tabulated.

Welded cold-rolled sheet — tested postweld treatment

Room-temperature mechanical properties
PropertyTypical valueUnit
Tensile strength1115MPa
0.1% proof stress752MPa
0.2% proof stress794MPa
Elongation17%

Table 12; 20°C. 2–3 min at 1150°C, fluidized-bed quench; weld; 20 min at 1040°C, air cool; 4 h at 750°C, air cool. Elongation gauge: 50 mm. Average/typical results, not acceptance minima. Hardness not tabulated.

Cold-forming sheet — solution annealed only

Annealed sheet forming properties
PropertyTypical valueUnit
Tensile strength865MPa
0.1% proof stress434MPa
0.2% proof stress461MPa
0.5% proof stress484MPa
Elongation on 50 mm50.0%
Hardness243HV

Bulletin p17: 0.6–2.0 mm sheet, 2–3 min/1150°C/fluidized-bed quench. Test temperature and hardness load not explicitly stated; not a verified 20°C test row. Reduction of area not tabulated.

Tabulated producer data only. Preserve form and heat treatment when comparing values.

Extruded bar — solution treated and aged — elevated-temperature tensile

Extruded bar — solution treated and aged — elevated-temperature tensile
Temperature (°C)UTS (MPa)0.1% proof (MPa)0.2% proof (MPa)Elongation (%)Reduction of area (%)
10011487237422746
20011116897082846
30010876646812948
40010816616783249
50010386576723149
60010276576752647
7008996216401828
8006575105321826
9003492883063051
100076454813099

Table 8. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.

Extruded bar subsequently forged — solution treated and aged — elevated-temperature tensile

Extruded bar subsequently forged — solution treated and aged — elevated-temperature tensile
Temperature (°C)UTS (MPa)0.1% proof (MPa)0.2% proof (MPa)Elongation (%)Reduction of area (%)
10012027577772642
20011757327512642
30011697157342843
40011487157322844
50011207067262843
60010926987232339
7009656907111317
8006835515731016
9003462843002137
10007645487797

Table 9. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.

Extruded section subsequently cold rolled — solution treated and aged — elevated-temperature tensile

Extruded section subsequently cold rolled — solution treated and aged — elevated-temperature tensile
Temperature (°C)UTS (MPa)0.1% proof (MPa)0.2% proof (MPa)Elongation (%)Reduction of area (%)
10012337918132843
20012037627772945
30012037427603045
40011897327483344
50011347267452941
60011357177482541
7009867037222222
8007175735982326
9003883323493446
100091505413297

Table 10. 8 h at 1080°C, air cool; 16 h at 700°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.

Cold-rolled sheet — tested three-stage treatment — elevated-temperature tensile

Cold-rolled sheet — tested three-stage treatment — elevated-temperature tensile
Temperature (°C)UTS (MPa)0.1% proof (MPa)0.2% proof (MPa)Elongation (%)
100113876479124
200110475478026
300107274175427
400103873475428
50099571774030
60096170172923
7008486807038
8006695055486
90034627228916
100083576266

Table 11. 2–3 min at 1150°C, fluidized-bed quench; 20 min at 1040°C, air cool; 4 h at 750°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.

Welded cold-rolled sheet — tested postweld treatment — elevated-temperature tensile

Welded cold-rolled sheet — tested postweld treatment — elevated-temperature tensile
Temperature (°C)UTS (MPa)0.1% proof (MPa)0.2% proof (MPa)Elongation (%)
100110675478819
200106772275219
300102169573119
40099970372919
50095668171419
60092568070913
7008206807144
8006045385632
9003572913127
100096546246

Table 12. 2–3 min at 1150°C, fluidized-bed quench; weld; 20 min at 1040°C, air cool; 4 h at 750°C, air cool. Strain rate 0.002/min to proof, 0.1/min thereafter. Typical results, not design allowables. Representative producer data; not guaranteed specification limits.

Continuous air oxidation — 100 h

Continuous air oxidation — 100 h
Temperature (°C)Descaled weight loss (mg/cm²)
8000.46
9002.52
9505.5
100010.4
110011.23

Producer p. 17. Exposure test, not service-temperature qualification. Representative producer data; not guaranteed specification limits.

Oxidation performance

  • See the 100 h continuous-air test table. Intermittent and cyclic data are distinct tests and must not be combined.

No graph estimates. Creep-rupture analysis tables, including source extrapolation flags, are retained in the technical review notes, not promoted here to guaranteed properties. No producer spring stress-relaxation conditions verified; no spring maximum operating temperature asserted. Suitability depends on stress, temperature, exposure duration, atmosphere and required service life; test temperatures are not universal service ratings.

Bar — recommended

8 h at 1080°C, air cool; 16 h at 700°C, air cool.

Sheet — recommended

3 min/1150°C/FBQ or WQ + 1 h/925°C/AC + 4 h/750°C/AC.

Welded sheet — recommended

3 min/1150°C/FBQ or WQ + weld + 1 h/925°C/AC + 4 h/750°C/AC.

Sheet interstage anneal

20 min/1040°C/AC or WQ.

Recommended sheet treatment differs from actual tensile-table treatment using 1040°C second stage. Do not reassign those measured properties to the 925°C route.

Material selection

Corrosion resistance & performance

Oxidation performance depends on exposure cycle, atmosphere, time and temperature; no unconditional operating-temperature rating is implied.

Typical applications

Engineering applications

  • Turbine blades
  • Turbine discs
  • Forgings
  • Ring sections
  • Hot-working tools

Subsequent manufacturing

Machining & processing

Hot working

1050–1200°C.

Machining

Machine fully heat treated. Producer prose hardness range 250–350 HV. This is not a condition-specific tabulated hardness guarantee.

Welding

Sheet resistance welding and TIG/MIG to about 5 mm are supported; thicker fusion welds risk microfissuring. Weld solution-treated material and postweld heat treat.

Material certification & testing

Certification and inspection options are subject to customer requirements and supplier confirmation.

Conformity must be demonstrated against the ordered specification, form and condition. Tests are not automatic; agree scope, acceptance criteria and documentation before ordering.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

Nimonic 90 Nickel Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.