Materials Supply / Alloy & High-Strength Steels
4130 Chromium-Molybdenum Steel
SAE / AISI 4130 | UNS G41300 | Cr–Mo low-alloy steel
4130 is a chromium–molybdenum low-alloy steel used where strength, toughness and fabrication capability must be balanced. “Chrome-moly” and “chromoly” are family descriptions, not exclusive grade names or complete purchase specifications.
Product form, section, melting route and heat treatment control delivered properties. The numerical data below are historical NASA measured averages for 25.4 mm bar, not producer acceptance limits or universal 4130 values.
Imagery is illustrative steel product forms, not certified 4130 stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
SAE specifications verify bars, forgings, rings, flat products and seamless tubing in distinct conditions; Metallus lists 4130 in its melted-grade portfolio. Every dimension, condition and specification remains subject to supplier confirmation at enquiry; no stockholding is implied.
- Bar and forging stock
- Forgings and flash-welded rings
- Sheet, strip and plate
- Seamless mechanical tubing
Material overview
4130 Chromium-Molybdenum Steel
A nominally 0.30% carbon chromium–molybdenum steel supplied in many forms and heat-treatment conditions, not one fixed strength level.
- Reference chemistry is approximately 0.30% carbon with controlled chromium and molybdenum; H, RH, HW and modified variants can have different requirements.
- AMS6370 covers bars, forgings and rings; AMS6345 covers normalized or otherwise heat-treated flat products up to 38.10 mm. Neither scope should be transferred to tubing.
- AMS6360, AMS6361 and AMS6371 are separate seamless-tubing specifications. AMS6361H identifies a 125 ksi (862 MPa) tensile condition that does not automatically apply to the others.
- The two NASA conditions demonstrate the effect of tempering on strength and impact energy; they are not specification minima or a complete heat-treatment guide.
Designations and product specifications
| Designation / standard | Scope and qualification |
|---|---|
| SAE / AISI | 4130 |
| UNS | G41300 — official registry entry not directly inspected |
| AMS6370S (2025) | Aircraft-quality bars, forgings, flash-welded rings and associated stock; not sheet or tubing |
| AMS6345F (2024) | Aircraft-quality sheet, strip and plate, normalized or otherwise heat treated, up to 38.10 mm (1.500 in) |
| AMS6348 | Normalized bars; current revision and complete condition requirements not independently resolved |
| AMS6350 | Annealed sheet, strip and plate reference; current revision and full scope require confirmation |
| AMS6360 / AMS6361 / AMS6371 | Distinct seamless-tubing specifications. AMS6361H (2024) covers round seamless tubing at 125 ksi (862 MPa) tensile strength; do not transfer this condition |
| ASTM A322-24 | Hot-wrought standard-grade alloy bars; confirm grade inclusion and ordered requirements in the full table |
| ASTM A519/A519M-24a | Hot- or cold-finished seamless carbon and alloy mechanical tubing; confirm grade and dimensions |
| SAE J404 | Chemical-composition reference only; not a complete product, aerospace-quality or mechanical acceptance specification |
Specifications are form- and condition-specific and are not interchangeable. Public catalogue scopes do not expose every chemistry, sampling, dimension or acceptance clause. Obtain the controlled revision required by the purchase order; historical or distributor cross-references do not establish certification.
ANSI / SAE — AMS6370S (2025), aircraft-quality 4130 bars, forgings, rings and stock
Specification review
Technical verification requirements
Physical properties and current standards
No exact-grade primary physical dataset was verified; several full AMS revision clauses remain inaccessible.
Obtain the controlled ordered specifications and a matching producer datasheet before technical approval.
Mechanical evidence
Numerical properties are 1973 NASA measured averages for one bar size and two tempers, not producer acceptance limits.
Confirm supplier condition-specific minima, section limits and test requirements for the intended product.
Grade selection
4130, 4140 and 8740 — selection distinctions
| Aspect | 4130 | 4140 | 8740 |
|---|---|---|---|
| Alloy system | Chromium–molybdenum | Chromium–molybdenum | Nickel–chromium–molybdenum |
| Carbon reference range | 0.28–0.33% | 0.38–0.43% | 0.38–0.43% |
| Manganese reference range | 0.40–0.60% | 0.75–1.00% | 0.75–1.00% |
| Nickel reference range | 0.25% maximum residual note | 0.25% maximum residual note | 0.40–0.70% deliberate addition |
| Chromium / molybdenum | 0.80–1.10% / 0.15–0.25% | 0.80–1.10% / 0.15–0.25% | 0.40–0.60% / 0.20–0.30% |
| Fabrication starting point | Lower-carbon Cr–Mo grade; welding still requires qualification | Higher-carbon Cr–Mo grade; preheat and post-weld assessment are more demanding | Not a routine welded-fabrication substitute for 4130 |
Reference chemistry from the TimkenSteel handbook, not a merged acceptance specification. The NASA results on each page are measured at different tempers and do not establish a universal strength or toughness ranking. Compare actual section, condition, orientation and ordered tests. 8740 is not 4340: its nickel range is much lower.
Engineering reference
Technical data
| Element | Minimum mass % | Maximum mass % |
|---|---|---|
| Carbon | 0.28 | 0.33 |
| Manganese | 0.40 | 0.60 |
| Silicon | 0.15 | 0.35 |
| Chromium | 0.80 | 1.10 |
| Nickel — residual note | — | 0.25 |
| Molybdenum | 0.15 | 0.25 |
| Phosphorus — general note | — | 0.035 |
| Sulphur — general note | — | 0.040 |
| Iron | Balance | Balance |
TimkenSteel Practical Data for Metallurgists, 18th edition, printed pages 6–7 and table general notes. Reference composition limits, not a typical heat analysis, product-analysis tolerance or declaration of compliance with every AMS/ASTM edition. Confirm the selected purchase specification and heat certificate.
| Property | Verified value | Qualification |
|---|---|---|
| Grade-specific physical-property dataset | Not verified from an exact-grade primary source | Generic steel values and modified SAE4130m data are not substituted |
No density, modulus, thermal conductivity, expansion, specific heat or resistivity is invented for 4130. Obtain a producer datasheet tied to the actual product and condition before adding design values.
NASA 25.4 mm bar — 30 HRC — 566°C temper
| Property | Measured average | Test / condition basis |
|---|---|---|
| Hardness | 30 HRC | Measured after the stated treatment |
| Ultimate tensile strength | 906 MPa | Average of five smooth longitudinal specimens |
| 0.2% offset yield strength | 774 MPa | Average of five smooth longitudinal specimens |
| Elongation | 22.1% | 50.8 mm (2.0 in) gauge length |
| Reduction of area | 69.4% | Longitudinal round tensile specimen |
| Charpy V impact energy | 151.4 J | Mean; 5 room-temperature tests; MIL-STD-151 specimen |
NASA TM X-64791 (1973), Tables II–VII. Approximately 25.4 mm (1.0 in) diameter bar; longitudinal specimens tested at 26.7°C (80°F). Treatment: normalized 899°C, austenitized 866°C, tempered 566°C; oil quenched before tempering. Soak times and Charpy notch orientation were not resolved. Historical measured averages, not producer guarantees, specification minima or design allowables.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
NASA 25.4 mm bar — 37 HRC — 385°C temper
| Property | Measured average | Test / condition basis |
|---|---|---|
| Hardness | 37 HRC | Measured after the stated treatment |
| Ultimate tensile strength | 1,133 MPa | Average of five smooth longitudinal specimens |
| 0.2% offset yield strength | 940 MPa | Average of five smooth longitudinal specimens |
| Elongation | 16.8% | 50.8 mm (2.0 in) gauge length |
| Reduction of area | 63.2% | Longitudinal round tensile specimen |
| Charpy V impact energy | 37.0 J | Mean; 5 room-temperature tests; MIL-STD-151 specimen |
NASA TM X-64791 (1973), Tables II–VII. Approximately 25.4 mm (1.0 in) diameter bar; longitudinal specimens tested at 26.7°C (80°F). Treatment: normalized 899°C, austenitized 866°C, tempered 385°C; oil quenched before tempering. Soak times and Charpy notch orientation were not resolved. Historical measured averages, not producer guarantees, specification minima or design allowables.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
Documented NASA experimental route
Normalize at 899°C, austenitize at 866°C, oil quench, then temper at 566°C or 385°C to produce the two reported 25.4 mm bar conditions. Soak times were not supplied.
Production heat treatment
Normalize, anneal, or quench and temper according to the ordered product specification, ruling section and qualified procedure. The experimental cycle is not a universal production recipe.
Modified-grade exclusion
Ovako SAE4130m / 34CrMo4 hardness data are not used because that producer expressly identifies chemistry deviations from standard ASTM A29 4130.
Condition and section must accompany every property requirement. Do not infer specification acceptance values from the NASA measured averages or transfer modified-grade data to standard 4130.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
Typical applications
Engineering applications
- Welded tubular structures, subject to procedure approval
- Aircraft engine mounts and structural fittings, where specified
- Shafts and high-integrity engineering components
- Selected oilfield components to the required service specification
Subsequent manufacturing
Machining & processing
Welding
The lower carbon content provides a different fabrication starting point from 4140, but no “weldable without preheat” claim is made. Qualify chemistry, wall thickness, restraint, hydrogen control, preheat and post-weld treatment.
Machining and forming
Procure an annealed, normalized or other agreed condition suitable for the manufacturing route. Welding or subsequent heat treatment can change the original strength and HAZ hardness.
Specification selection
State product form, condition, section and required tests together. A sheet, bar or tube carrying the same SAE grade name does not share one acceptance specification.
Applications
Aerospace, pressure-service and oilfield uses require the applicable component and material approvals; ordinary commercial 4130 is not automatically qualified.
Material certification & testing
Documentation and inspection must be agreed for the actual grade name, specification revision, melting route, product form, ruling section and delivery condition.
No certificate, test, aerospace approval or grade equivalence is automatic. The short names 4330V and 4330M are not sufficient procurement specifications; quotation controls remain disabled.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Heat / batch traceability to the producing mill
- Chemical analysis and mechanical test reports to the ordered specification
- Heat-treatment records identifying the complete cycle and load, where required
- Melting / remelting-route evidence, ultrasonic inspection, PMI or customer-specific testing only where agreed
Material enquiry
Request a material quotation
4130 Chromium-Molybdenum Steel supplied to your material form, dimensions and specification.