Materials Supply / Alloy & High-Strength Steels
8740 Nickel-Chromium-Molybdenum Steel
SAE / AISI 8740 | UNS G87400 | Ni–Cr–Mo low-alloy steel
8740 is a nickel–chromium–molybdenum low-alloy steel used in heat-treated high-strength components. Its deliberate nickel addition distinguishes it from 4140, while its much lower nickel range distinguishes it from 4340.
TimkenSteel lists 8740 among “Formerly Standard Steels”; this does not make it obsolete, as modern AMS6322 and AMS6325 editions remain catalogued. Chemistry and mechanical properties still require the selected specification and condition.
Imagery is illustrative steel product forms, not certified 8740 stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
AMS6322 verifies bars, forgings, rings and stock; AMS6325 covers heat-treated bars and forgings, and SAE lists AMS6358 for flat products. No current producer catalogue proving specific tubing, wire or stock dimensions was verified. Confirm all forms and availability at enquiry.
- Bar and forging stock
- Forgings and flash-welded rings
- Sheet, strip and plate — specification enquiry
Material overview
8740 Nickel-Chromium-Molybdenum Steel
A nominally 0.40% carbon nickel–chromium–molybdenum steel for heat-treated components, distinct from both 4140 and higher-nickel 4340.
- Reference carbon and manganese ranges match 4140, but 8740 uses lower chromium, deliberate nickel and a higher molybdenum range. Neither grade is universally stronger or tougher without matched conditions.
- AMS6325M identifies a heat-treated 105 ksi (724 MPa) tensile-strength condition for bars and forgings. This title condition is not a universal typical UTS for 8740.
- The two NASA 25.4 mm bar datasets are measured averages at 28 and 40 HRC. They are not specification acceptance limits or design allowables.
- 8740 is not 8640, 4340 or a modified 8740 variant. H/RH hardenability-controlled and proprietary variants require their own chemistry and specification review.
Designations and product specifications
| Designation / standard | Scope and qualification |
|---|---|
| SAE / AISI | 8740 |
| UNS | G87400 — official registry entry not directly inspected |
| AMS6322S (2023) | Aircraft-quality bars, forgings, flash-welded rings and associated stock |
| AMS6325M (2024) | Aircraft-quality heat-treated bars and forgings, 105 ksi (724 MPa) tensile-strength condition; full dimensions and acceptance clauses required |
| AMS6358 | Sheet, strip and plate; SAE lists 6358L (2020) as latest revised. Present producer availability and complete requirements not verified |
| ASTM A322-24 | Hot-wrought standard-grade alloy bars; confirm 8740 inclusion and purchase requirements in the full table |
| SAE J404 | Chemistry reference only; current grade-table inclusion and full product requirements must be checked |
| Excluded generic standards | ASTM A334 low-temperature tube and withdrawn A331 are not current generic 8740 acceptance specifications |
Product specifications are not interchangeable across form and condition. TimkenSteel’s “Formerly Standard Steels” label is not a cancellation statement. Obtain controlled current standards and supplier-confirmed forms; no wire or tubing coverage is inferred.
SAE AMS6322S — aircraft-quality 8740 bars, forgings, rings and stock (2023)
Specification review
Technical verification requirements
Chemistry and physical data
Silicon comes from a separate AMS6322 handbook table; universal P/S limits and exact-grade physical properties were not verified.
Obtain the complete ordered chemistry and matching producer physical datasheet rather than merging legacy tables.
Supply and mechanical evidence
Current producer stock forms/dimensions were not established; numerical mechanics are 1973 NASA averages for two experimental conditions.
Confirm present supplier forms, condition-specific acceptance limits and required component tests before technical approval.
Grade selection
4130, 4140 and 8740 — selection distinctions
| Aspect | 4130 | 4140 | 8740 |
|---|---|---|---|
| Alloy system | Chromium–molybdenum | Chromium–molybdenum | Nickel–chromium–molybdenum |
| Carbon reference range | 0.28–0.33% | 0.38–0.43% | 0.38–0.43% |
| Manganese reference range | 0.40–0.60% | 0.75–1.00% | 0.75–1.00% |
| Nickel reference range | 0.25% maximum residual note | 0.25% maximum residual note | 0.40–0.70% deliberate addition |
| Chromium / molybdenum | 0.80–1.10% / 0.15–0.25% | 0.80–1.10% / 0.15–0.25% | 0.40–0.60% / 0.20–0.30% |
| Fabrication starting point | Lower-carbon Cr–Mo grade; welding still requires qualification | Higher-carbon Cr–Mo grade; preheat and post-weld assessment are more demanding | Not a routine welded-fabrication substitute for 4130 |
Reference chemistry from the TimkenSteel handbook, not a merged acceptance specification. The NASA results on each page are measured at different tempers and do not establish a universal strength or toughness ranking. Compare actual section, condition, orientation and ordered tests. 8740 is not 4340: its nickel range is much lower.
Engineering reference
Technical data
| Element | Minimum mass % | Maximum mass % |
|---|---|---|
| Carbon | 0.38 | 0.43 |
| Manganese | 0.75 | 1.00 |
| Silicon — AMS6322 cross-reference table | 0.15 | 0.35 |
| Chromium | 0.40 | 0.60 |
| Nickel | 0.40 | 0.70 |
| Molybdenum | 0.20 | 0.30 |
| Iron | Balance | Balance |
Main C/Mn/Cr/Ni/Mo ranges come from TimkenSteel’s “Formerly Standard Steels” table; silicon is from its separate AMS6322 cross-reference table. Phosphorus and sulphur are specification-dependent and deliberately not merged from a different legacy military table. Obtain the ordered specification for a complete acceptance chemistry and product-analysis tolerances.
| Property | Verified value | Qualification |
|---|---|---|
| Grade-specific physical-property dataset | Not verified from an exact-grade primary producer source | Secondary generic-steel values are not substituted |
No density, modulus, thermal conductivity, expansion, specific heat or resistivity is invented for 8740. Obtain an exact-grade producer datasheet and its condition/temperature basis before adding design values.
NASA 25.4 mm bar — 28 HRC — 635°C temper
| Property | Measured average | Test / condition basis |
|---|---|---|
| Hardness | 28 HRC | Measured after the stated treatment |
| Ultimate tensile strength | 906 MPa | Average of five smooth longitudinal specimens |
| 0.2% offset yield strength | 822 MPa | Average of five smooth longitudinal specimens |
| Elongation | 23.0% | 50.8 mm (2.0 in) gauge length |
| Reduction of area | 65.1% | Longitudinal round tensile specimen |
| Charpy V impact energy | 133.9 J | Mean; 3 room-temperature tests; MIL-STD-151 specimen |
NASA TM X-64791 (1973), Tables II–VII. Approximately 25.4 mm (1.0 in) diameter bar; longitudinal specimens tested at 26.7°C (80°F). Treatment: normalized 899°C, austenitized 843°C, tempered 635°C; oil quenched before tempering. Soak times and Charpy notch orientation were not resolved. Historical measured averages, not producer guarantees, specification minima or design allowables.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
NASA 25.4 mm bar — 40 HRC — 454°C temper
| Property | Measured average | Test / condition basis |
|---|---|---|
| Hardness | 40 HRC | Measured after the stated treatment |
| Ultimate tensile strength | 1,271 MPa | Average of five smooth longitudinal specimens |
| 0.2% offset yield strength | 1,205 MPa | Average of five smooth longitudinal specimens |
| Elongation | 16.7% | 50.8 mm (2.0 in) gauge length |
| Reduction of area | 57.5% | Longitudinal round tensile specimen |
| Charpy V impact energy | 70.2 J | Mean; 3 room-temperature tests; MIL-STD-151 specimen |
NASA TM X-64791 (1973), Tables II–VII. Approximately 25.4 mm (1.0 in) diameter bar; longitudinal specimens tested at 26.7°C (80°F). Treatment: normalized 899°C, austenitized 843°C, tempered 454°C; oil quenched before tempering. Soak times and Charpy notch orientation were not resolved. Historical measured averages, not producer guarantees, specification minima or design allowables.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
NASA 28 HRC experimental condition
Normalize 899°C, austenitize 843°C, oil quench and temper at 635°C. Soak times were not supplied; this is the reported route for the 25.4 mm bar measurements.
NASA 40 HRC experimental condition
Normalize 899°C, austenitize 843°C, oil quench and temper at 454°C. Soak times were not supplied; this is a separate measured condition, not an alternative acceptance limit.
Production route
Procure an annealed or otherwise agreed machining/forming condition, then develop final properties using the applicable specification and a validated section-specific heat-treatment procedure.
NASA Table II gives 28 HRC for the lower-hardness 8740 condition; a narrative reference to Rc29 is not used. The experimental schedules are historical evidence, not universal production instructions.
NASA TM X-64791 — Low Temperature Mechanical Properties of Several Alloy Steels (November 1973), Tables II–VII
Typical applications
Engineering applications
- High-strength bolts, studs and fasteners to component specifications
- Aircraft-quality forged components, where approved
- Heat-treated high-strength engineering components
Subsequent manufacturing
Machining & processing
Machining and forming
Procure an annealed or agreed stock condition suitable for the manufacturing route, then apply controlled final heat treatment. Confirm actual hardness before selecting machining parameters.
Welding
Do not treat 8740 as a routine welded-fabrication substitute for 4130. Its carbon and alloy content warrant a qualified low-hydrogen procedure and explicit HAZ-cracking and post-weld-property assessment.
Fastener manufacture
High strength alone does not establish fatigue performance, plating suitability or hydrogen-embrittlement resistance. Control hardness, manufacturing route, surface treatment and component specification.
Application evidence
The listed applications are established selection categories, not claims of current producer stock or component approval. Confirm the intended product range and service requirements with the supplier.
Material certification & testing
Documentation and inspection must be agreed for the actual grade name, specification revision, melting route, product form, ruling section and delivery condition.
No certificate, test, aerospace approval or grade equivalence is automatic. The short names 4330V and 4330M are not sufficient procurement specifications; quotation controls remain disabled.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Heat / batch traceability to the producing mill
- Chemical analysis and mechanical test reports to the ordered specification
- Heat-treatment records identifying the complete cycle and load, where required
- Melting / remelting-route evidence, ultrasonic inspection, PMI or customer-specific testing only where agreed
Material enquiry
Request a material quotation
8740 Nickel-Chromium-Molybdenum Steel supplied to your material form, dimensions and specification.