Representative hot-rolled low-alloy steel round bars

Materials Supply / Alloy & High-Strength Steels

8620 Nickel-Chromium-Molybdenum Case-Hardening Steel

SAE / AISI 8620 | Ni–Cr–Mo case-carburising steel

8620 is a low-carbon nickel–chromium–molybdenum steel normally used in the carburised, hardened and tempered condition, where surface carbon enrichment produces a hard case and the low-carbon core retains toughness.

Its finished case and core properties depend on the carburising cycle, case depth, section size, quench and temper. No single “8620 mechanical properties” table applies to every component.

Imagery is illustrative steel product forms, not certified 8620 stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

AMS6274 covers aircraft-quality bars, forgings, mechanical tubing and forging stock; SSAB lists 8620 discrete plate 12.7–50.8 mm thick to ASTM A829. These are producer and specification scopes, not Quest stock. Confirm all forms, sizes and availability at enquiry.

  • Bar and forging stock
  • Forgings
  • Mechanical tubing
  • Plate — specification enquiry

Material overview

8620 Nickel-Chromium-Molybdenum Case-Hardening Steel

A low-carbon nickel–chromium–molybdenum steel carburised to give a hard wear-resistant case over a tougher core.

  • Supply-condition hardness, non-carburised hardened response and carburised case/component performance are separate questions and are presented separately here.
  • Air-melt aircraft-quality (AMS6274) and remelted premium-quality (AMS6276 VAR; AMS6277 VAR or ESR) material are distinct procurement routes.
  • 8620H is a hardenability-banded variant and is not assumed to be equivalent to plain 8620.

Designations and product specifications

Designations and product specifications
Designation / standardScope and qualification
SAE / AISI8620
UNSCommonly mapped to G86200 — official registry entry not directly inspected
AMS6274S (2021)Aircraft-quality bars, forgings, mechanical tubing and forging stock
AMS6276N (December 2025)Premium aircraft-quality, consumable-electrode vacuum remelted bars, forgings, tubing and stock
AMS6277Premium aircraft-quality, vacuum arc or electroslag remelted; current revision text not fully verified
ASTM A322-24 / A29/A29M-26Hot-wrought alloy bars / general bar requirements; confirm 8620 table entry in the full standard
ASTM A829/A829M-25Alloy structural steel plate
ASTM A519/A519M-24aSeamless mechanical tubing — product-form standard
SAE J404Chemistry reference only; full 8620 row not verified
Excluded referencesAMS6375 is welding wire; ASTM A331 (withdrawn 2004) and A752 (withdrawn 2011) are not current 8620 specifications

Similar European designations (20NiCrMo2-2, 1.6523) are listed by producers as similar, not identical; chemistry ranges differ. Obtain controlled current standards before ordering.

SAE AMS6274S — 8620 bars, forgings and tubing (23 July 2021)

Specification review

Technical verification requirements

  • Chemistry and specifications

    SAE J404, AMS6274/6276/6277 full chemistry tables were not accessed; SSAB plate limits and Ovako variant limits differ.

    Obtain the ordered specification revision and mill certificate chemistry.

  • Mechanical evidence

    No producer-qualified case/core tensile dataset was found; SSAB does not routinely test A829 plate mechanicals; voestalpine figures (850 MPa, 20 J, 11%) lack any test basis and are not used.

    Obtain qualified case/core test results for the actual carburising cycle, section and case depth.

  • Hardenability

    SAE J1268 8620H band and current revision were not verified.

    Specify 8620H and its band explicitly if hardenability control is required.

Grade selection

8620, 9310 and 52100 — different hardening principles

8620, 9310 and 52100 — different hardening principles
Aspect8620931052100
Hardening principleCase carburisingCase carburising (premium aerospace routes common)Through hardening — not a carburising steel
Carbon basis used here0.18–0.23% (SSAB plate limits)0.07–0.13% (Liberty AMS-referenced limits)1.00% (Carpenter nominal)
Nickel basis used here0.40–0.70%3.00–3.50%Not a deliberate addition (Ovako variants ≤0.25%)
Chromium basis used here0.40–0.60%1.00–1.40%1.40% (Carpenter nominal)
Key aerospace specificationsAMS6274 air melt; AMS6276 / AMS6277 remeltedAMS6260; AMS6265 VAR; AMS6267 ESR or VARAMS6440; AMS6444 VAR; ASTM A295
Published property basis on these pagesSupply hardness; one carburised research specimenTypical core properties after pseudo-carburisingAnnealed-bar tensile data; tempering-hardness response

Each value retains its own source basis; producer typical figures and specification-referenced limits are not interchangeable. 9315 (AMS6263) is a different grade from 9310. No universal fatigue, wear or toughness ranking is inferred; substitution requires engineering approval against the full specification, melt route, section, heat treatment and tests.

Engineering reference

Technical data

Chemical composition — SSAB 8620 plate heat-analysis limits
ElementMinimum mass %Maximum mass %
Carbon0.180.23
Manganese0.700.90
Silicon0.150.35
Chromium0.400.60
Nickel0.400.70
Molybdenum0.150.25
Phosphorus—0.030
Sulphur—0.030
IronBalanceBalance

SSAB heat-analysis limits for its A829 8620 plate, not a transcription of SAE J404 or any AMS specification. Ovako 20NiCrMo2-2 variants use different limits (e.g. 152A: Mn 0.65–0.90, Cr 0.40–0.70, S 0.020–0.035). Use the ordered specification for acceptance chemistry.

Physical properties — Ovako 20NiCrMo2-2 typical values
PropertyTypical valueTemperature basis as published
Density7800 kg/m³Not specified
Young’s modulus210 GPaNot specified
Shear modulus80 GPaNot specified
Poisson’s ratio0.3Not specified
Mean coefficient of thermal expansion12 µm/(m·K)20–300°C
Specific heat capacity460–480 J/(kg·K)Printed as 50/100°C
Thermal conductivity40–45 W/(m·K)Ambient
Electrical resistivity0.20–0.25 µΩ·mAmbient

Ovako states these values apply to Ovako material only; 8620 to other specifications need not have identical properties.

Ovako round bar — as rolled / soft annealed supply hardness

8620-similar 20NiCrMo2-2 — supply-condition hardness (typical)
Variant and dimension as printedAs rolledSoft annealed
152A, “40 < 80” mm round bar230 HB212 HB
152G, “40 < 70” mm round bar230 HB212 HB

Ovako typical supply-condition hardness, not carburised case or core hardness. Dimension notation retained as printed; sampling position and test load not stated. No tensile values are published for these supply conditions.

Carburised research specimen — 25 mm bar — single monotonic test

8620 — carburised specimen, University of Toledo / AISI (2004)
PropertyMeasured resultBasis
0.2% offset yield strength1125.3 MPaOne monotonic test, ASTM E8, room temperature
Ultimate tensile strength1868.7 MPaOne monotonic test
Elongation1.7%Gauge-length basis not established
Reduction of area0.1%One monotonic test
Modulus of elasticity207.9 GPaSame test
Hardness — grip surface61.5 HRCUnground flat grip section
Hardness — gauge-section centre58.2 HRCSmall specimen; not an isolated core test

Measured result for one carburised, ground and polished specimen of approximately 5 mm (0.20 in) minimum diameter, machined from ~25 mm MacSteel round bar. The heat’s Mn (0.96%) exceeds the SSAB limits above. The full carburising cycle and case-depth criterion were not established. Not core properties, typical values, specification minima or design allowables.

Yin & Fatemi, University of Toledo — SAE 8620 Carburized Case Steel, Iteration #71 (AISI Bar Steel Applications Group, April 2004)

Hot forging

800–1200°C, air cool.

Normalising

860–890°C, air cool.

Soft annealing

600–670°C for 2 h, air cool.

Carburising

850–930°C; carbon potential to suit the required case. Duration and case depth are component-specific.

Hardening

Quench and temper route 840–890°C; hardening of an as-carburised component 780–830°C; oil quench.

Tempering

160–250°C, air cool.

Ovako 20NiCrMo2-2 recommendations; no section size, quench-oil conditions, carburising duration, effective case depth or guaranteed case/core hardness accompanies them. Ovako graphs are theoretical-model outputs. A voestalpine datasheet prints “Temper 850–880°C”, an apparent error that is not reproduced. Qualify a section-specific procedure before production.

Typical applications

Engineering applications

  • Carburised gears and pinions
  • Shafts, splines and cam components requiring a wear-resistant surface
  • Aircraft-quality carburised components to AMS6274/6276/6277, where approved

Subsequent manufacturing

Machining & processing

Machining

Machine in the annealed or agreed supply condition before carburising; allow for grinding stock and distortion after hardening.

Case-depth specification

Specify effective case depth, its hardness criterion, surface and core hardness and the inspection method on the component drawing; the grade name does not define them.

Welding

Welding of carburised surfaces is not a routine operation. Any welding requires a qualified procedure and assessment of hardness and cracking risk.

Application evidence

Listed applications are established selection categories, not claims of stock or component approval.

Material certification & testing

Documentation and inspection must be agreed for the actual grade, specification revision, melting route, product form, ruling section and delivery condition.

No certificate, test, aerospace approval or grade equivalence is automatic. Case depth and case/core properties belong to the finished heat-treated component, not to the grade name; quotation controls remain disabled.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the producing mill
  • Chemical analysis and mechanical test reports to the ordered specification
  • Carburising, hardening and tempering records, case-depth and hardness-traverse reports where required
  • Melting-route, cleanliness, ultrasonic, PMI or customer-specific testing only where agreed

Material enquiry

Request a material quotation

8620 Nickel-Chromium-Molybdenum Case-Hardening Steel supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.