Representative extruded aluminium alloy round bars

Materials Supply / Aluminium Alloys

Aluminium Alloy 6061

Versatile heat-treatable Al–Mg–Si–Cu alloy for structural and precision engineering

6061 is a versatile precipitation-hardenable aluminium alloy used for structural components, machinery and precision-machined parts. Magnesium and silicon provide the principal age-hardening response, with controlled copper and chromium additions.

Rolled plate and extruded bar are not interchangeable property bases. T651 plate is stretch stress relieved; T6511 extrusions also permit minor final straightening. Generic commercial material is not automatically approved for aerospace service.

Illustrative aluminium materials and fabricated components, not certified alloy stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

Producer sources verify rolled sheet/plate and extruded solid/hollow profiles, rod, bar, seamless and structural tube/pipe. Forgings are referenced by the specialist supplier against dedicated AMS specifications. Availability and temper depend on product route and size; listed forms are enquiry options, not a stock commitment.

  • Plate
  • Sheet
  • Round bar / rod
  • Flat bar
  • Extruded profiles
  • Tube and pipe
  • Forgings — specification enquiry
  • Cut-to-size stock

Material overview

Aluminium Alloy 6061

6061 combines useful strength, corrosion resistance and weldability in rolled and extruded products; specify product form, temper, section size and certification together.

  • The alloy sits within the 6000 Series — Heat-Treatable family. Solution treatment brings soluble constituents into solution; quenching retains a supersaturated matrix. Natural ageing and controlled artificial ageing develop Mg–Si-rich strengthening precipitates. The precipitation sequence, quench response and final properties depend on alloy chemistry and section size.
  • Quenching also introduces residual stress. Controlled stretching reduces that stress in T651 and T6511 products, improving machining stability without guaranteeing distortion-free parts. T6 does not by itself specify stretch stress relief.
  • Use producer minima only within their documented scope. Typical values are informative, not specification minima, MMPDS design allowables or guaranteed welded-joint properties.

Designation and specification references

Designation and specification references
ReferenceVerified product/temper association
AA 6061Registered wrought alloy; chemistry controlled separately by AA Teal Sheets
EN AW-6061 / AlMg1SiCuEuropean alloy designation; not a numeric steel material number or a blanket equivalence.
AMS 40256061-O sheet and plate
AMS 40266061-T4 sheet / T451 plate
AMS 40276061-T6 sheet / T651 plate
AMS 41736061-T6511 extrusion
AMS 4127 / AMS 4146T6 forgings / T4 forgings, respectively

Supplier cross-reference only, not a claim of compliance or current standard revision. Confirm the exact current specification, product dimensions, temper and test requirements at enquiry; no equivalence or automatic substitution is implied.

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

Grade selection

6061, 6063 and 6082 compared

6061, 6063 and 6082 compared
Aspect606160636082
Registered Mg / Si, mass %Mg 0.8–1.2 / Si 0.40–0.8Mg 0.45–0.9 / Si 0.20–0.6Mg 0.6–1.2 / Si 0.7–1.3
Principal additional elementsCu 0.15–0.40%; Cr 0.04–0.35%; Mn ≤0.15%Cu, Cr and Mn each ≤0.10%Mn 0.40–1.0%; Cr ≤0.25%; Cu ≤0.10%
Metallurgical classificationPrecipitation-hardenable Al-Mg-Si-Cu-CrPrecipitation-hardenable Al-Mg-SiPrecipitation-hardenable Al-Mg-Si-Mn
Common temper distinctionsT4 natural ageing; T6 artificial ageing; T651/T6511 include specified stress reliefT5 cooling from shaping then artificial ageing; T6 separate solution heat treatment and artificial ageingT4/T6 and stress-relieved product conditions depend on mill and product specification
Strength selectionEngineering strength depends on form, section and temperOften selected for extrusion quality rather than maximum strengthStructural strength depends on form, section and temper; not universally stronger than 6061
Extrudability and surface finishStructural and precision extrusion productsGood extrudability and surface finish; anodising quality still requires surface/process controlStructural extrusions; surface expectations require mill confirmation
MachinabilityAged tempers suited to machining; stress-relieved stock can reduce movementSofter tempers require chip and finish controlAged structural products suited to machining; residual stress still matters
Welding and formingWelding can soften aged HAZ; softer conditions improve formingGood weldability; HAZ and joint strength are not parent T5/T6 strengthWelding can soften aged HAZ; qualify joint properties
Corrosion protectionGood general resistance, not universal seawater immunityOften selected for corrosion resistance and anodised finishGood general resistance; coastal suitability remains environment-specific
Typical product focusSheet/plate, bar and extrusions subject to ordered requirementsExtruded profiles, bar and tubeEuropean structural plate, bar and extrusions
Engineering usesMachined parts, fixtures and structural fittingsFrames, enclosures, profiles and finished extrusionsStructural and transport components and machined equipment
Specification substitutionCommercial designation is not aerospace AMS approvalExtrusion-specific requirements are not plate requirementsCannot automatically replace 6061 on an AMS-controlled drawing

Qualitative selection guide, using registered AA chemistry and the grade-specific producer references on these pages. No numerical strength ranking: temper, product form, section size and test basis are not matched. No alloy or temper is automatically interchangeable; confirm the drawing and ordered specification.

The Aluminum Association — Teal Sheets, December 2025; fabrication references on each grade page

Engineering reference

Technical data

Chemical composition limits — 6061 (AA)
ElementMass %Limit
Si0.40–0.8Range
Fe0.7Maximum
Cu0.15–0.40Range
Mn0.15Maximum
Mg0.8–1.2Range
Cr0.04–0.35Range
Zn0.25Maximum
Ti0.15Maximum
Other elements, each0.05Maximum
Other elements, total0.15Maximum
AlRemainderBalance

Registered AA limits, not nominal or certified heat analysis. Ranges show minimum–maximum; all other numeric entries are maxima. AA other-element provisions apply. EN requirements are not independently merged into this table; agree the governing chemistry standard and mill certificate. Separately registered suffix alloys are not included.

The Aluminum Association — Teal Sheets, December 2025

Typical physical properties — rolled-product producer data
PropertyTypical valueCondition / temperature basis
Density2.70 Mg/m³Nominal, 20°C
Melting range582–652°CAlloy range; not a service-temperature rating
Specific heat896 J/(kg·K)100°C
Mean linear thermal expansion23.6 × 10⁻⁶ K⁻¹20–100°C
Thermal conductivity180 W/(m·K)O, 20°C
Thermal conductivity154 W/(m·K)T451, 20°C
Thermal conductivity167 W/(m·K)T6 / T651, 20°C
Elastic modulus68.3 GPaT6 / T651 typical mechanical table; temperature unstated

Typical values, not procurement acceptance limits. Temper and temperature are retained where specified. The source prints 68.3 GPa; retained without silently replacing it with the common rounded 69 GPa value. Electrical conductivity %IACS is omitted from this SI table rather than silently converted.

O — extruded products

O — extruded products
Specimen-section thicknessTensile strength (MPa)0.2% proof strength (MPa)Elongation (%)
All thicknesses150 maximum110 maximum16 minimum

Hydro North America extruded products; cross-section thickness at the tensile specimen determines the applicable properties. Producer limits, not typical values. Test temperature and orientation are not stated in this datasheet; no elevated-temperature basis is claimed. Elongation is measured in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. No upper thickness limit is specified by this table; confirm actual size capability and ordered specification.

T4 — extruded products

T4 — extruded products
Specimen-section thicknessTensile strength (MPa)0.2% proof strength (MPa)Elongation (%)
All thicknesses180 minimum110 minimum16 minimum

Hydro North America extruded products; cross-section thickness at the tensile specimen determines the applicable properties. Producer limits, not typical values. Test temperature and orientation are not stated in this datasheet; no elevated-temperature basis is claimed. Elongation is measured in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. No upper thickness limit is specified by this table; confirm actual size capability and ordered specification.

T6 — extruded products

T6 — extruded products
Specimen-section thicknessTensile strength (MPa)0.2% proof strength (MPa)Elongation (%)
Up through 0.249 in (up through 6.30 mm)260 minimum240 minimum8 minimum
0.250 in and above (>6.30 mm in source)260 minimum240 minimum10 minimum

Hydro North America extruded products; cross-section thickness at the tensile specimen determines the applicable properties. Producer limits, not typical values. Test temperature and orientation are not stated in this datasheet; no elevated-temperature basis is claimed. Elongation is measured in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. No upper thickness limit is specified by this table; confirm actual size capability and ordered specification.

T6511 — extruded products

T6511 — extruded products
Specimen-section thicknessTensile strength (MPa)0.2% proof strength (MPa)Elongation (%)
Up through 0.249 in (up through 6.30 mm)260 minimum240 minimum8 minimum
0.250 in and above (>6.30 mm in source)260 minimum240 minimum10 minimum

Hydro North America extruded products; cross-section thickness at the tensile specimen determines the applicable properties. Producer limits, not typical values. Test temperature and orientation are not stated in this datasheet; no elevated-temperature basis is claimed. Elongation is measured in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. No upper thickness limit is specified by this table; confirm actual size capability and ordered specification.

T6 — Kaiser typical specimen data

T6 — Kaiser typical specimen data
PropertyTypical valueBasis
Tensile strength310 MPa0.500 in diameter tensile specimen
Yield strength276 MPaOffset not specified in this table
Elongation17%4D gauge length
Brinell hardness95500 kg load; 10 mm ball
Ultimate shear strength207 MPaTypical

Kaiser publishes a shared T6/T651 row; reproduced separately without implying identical processing. Typical values only, not acceptance minima or design allowables. Published in the sheet/coil/plate datasheet, but the table is screw-machine-style typical stock data with a 0.500 inch diameter specimen; no specific product, thickness, orientation or test temperature is stated. Do not treat as a plate guarantee. Numerical fatigue data are omitted because the extracted cycle-count notation requires confirmation.

T651 — Kaiser typical specimen data

T651 — Kaiser typical specimen data
PropertyTypical valueBasis
Tensile strength310 MPa0.500 in diameter tensile specimen
Yield strength276 MPaOffset not specified in this table
Elongation17%4D gauge length
Brinell hardness95500 kg load; 10 mm ball
Ultimate shear strength207 MPaTypical

Kaiser publishes a shared T6/T651 row; reproduced separately without implying identical processing. Typical values only, not acceptance minima or design allowables. Published in the sheet/coil/plate datasheet, but the table is screw-machine-style typical stock data with a 0.500 inch diameter specimen; no specific product, thickness, orientation or test temperature is stated. Do not treat as a plate guarantee. Numerical fatigue data are omitted because the extracted cycle-count notation requires confirmation.

T651 — rolled products producer minima

T651 — rolled products producer minima
PropertyProducer minimumScope limitation
Tensile strength290 MPaRolled products; thickness not stated
0.2% proof strength240 MPaRolled products; thickness not stated
Elongation10%Gauge length not stated

Independent producer minima. This one-page rolled-products sheet does not state thickness range, orientation, test temperature, gauge length or governing mechanical standard. Do not apply to an arbitrary plate thickness without mill confirmation. Its fatigue/hardness cells contain apparent unit or layout errors and are deliberately excluded.

O — annealed

Annealed to the lowest-strength temper; useful for more severe forming. Hydro supplies a separate O extrusion property basis.

T4 — solution treated and naturally aged

Natural ageing follows solution heat treatment and quenching. This softer condition can support forming before subsequent controlled ageing; do not assume a shop operation automatically certifies T6.

T6 — solution treated and artificially aged

Artificial ageing develops strength through precipitation. No stretching requirement is inherent in T6. Section thickness, quench effectiveness and the applicable specification govern achieved properties.

T651 — stretch stress relieved and artificially aged

Solution heat treated, stress relieved by controlled stretching and artificially aged; the additional digits specify processing beyond T6. Typically selected for machined rolled plate. Stretch relief reduces but does not eliminate residual stress.

T6511 — extrusion stress-relief scope

Solution heat treated, stress relieved by stretching and artificially aged. The extrusion suffix permits minor straightening after stretching to meet dimensional tolerances. The Aluminum Association interpretation specifies no numerical range for that corrective straightening.

T5 is not T6

T5 means cooled from an elevated-temperature shaping process and artificially aged; it is not synonymous with solution-treated T6. No 6061-T5 condition or transferable mechanical values are offered here.

Hydro verifies 6061 O/T4/T6/T6511 definitions and stretch relief; AA interpretation of T_511: https://www.aluminum.org/sites/default/files/2023-12/Respone_to_questionnaire_about_TX511.pdf. No furnace temperatures, soak times, quench delays, permanent-set percentages or ageing schedules are prescribed here. Obtain a qualified product-specific procedure and required certification. Do not relabel a machined or welded component with a parent-stock temper without qualification.

Material selection

Corrosion resistance & performance

Hydro describes excellent atmospheric and good seawater corrosion resistance. These are qualitative producer statements, not immunity to pitting, crevice attack or corrosion fatigue. Consider drainage, deposits, chloride exposure and protective finishes.

Avoid uncontrolled direct contact with dissimilar metals; use appropriate isolation to limit galvanic corrosion.

6061 responds well to anodising, including clear, dyed and hardcoat finishes. For demanding cosmetic appearance Hydro suggests considering 6063; finish quality still depends on stock and processing.

Pitting, intergranular attack and stress-corrosion suitability require exposure-, temper- and product-specific assessment. Anodising or conversion coatings and galvanic isolation should be selected for the actual environment; these pages give no universal seawater or corrosion-life guarantee.

Typical applications

Engineering applications

  • Precision-machined brackets, fittings, housings and fixtures with product-specific strength requirements.
  • Structural frames, machinery and equipment components.
  • Transportation and recreational equipment components.
  • Welded engineering assemblies designed using qualified joint properties.
  • Aerospace components only where drawing, product specification, procurement and traceability requirements are explicitly satisfied.

Subsequent manufacturing

Machining & processing

Machining and dimensional stability

Hydro rates T6/T6511 as adequate for screw-machine applications. Turning and drilling chips may be difficult to break; chip breakers and peck drilling can help. Stress-relieved stock is useful for precision machining, but balanced material removal, workholding and intermediate inspection remain important.

Forming

O offers the best forming response; T4 is generally more formable than T6. Bend feasibility depends on radius, direction, thickness and section geometry. Hydro identifies softer tempers for severe bends; do not transfer one section’s bend capability to another.

Welding and joining

6061 can be welded by established commercial methods, but T6-strength material softens in the weld region and heat-affected zone. Parent-stock tensile values do not establish as-welded joint strength. Select filler and qualify the welding procedure for strength, corrosion and finish requirements; no universal post-weld heat-treatment schedule is asserted.

Fatigue and cyclic loading

Numerical fatigue values are omitted pending confirmation of the source cycle-count notation and specimen basis. Geometry, surface finish, notches, mean stress, corrosion and welds affect component life; no guaranteed endurance threshold or design allowable is given.

Thermal exposure

Heating can change the age-hardening condition and reduce strength or stability. Melting range is not a usable continuous-service limit. No verified numerical elevated-temperature design dataset is supplied here.

Thermal exposure and dimensional control

Natural and artificial ageing, quench rate and section thickness affect precipitate development and residual stress. Prolonged heating may overage the material; no maximum service temperature or numerical high-temperature design allowable is asserted. Plan machining, clamping and welding sequences to control distortion; post-weld heat treatment must be qualified rather than assumed to restore parent strength.

Material certification & testing

Order by alloy, exact product form, dimensions, temper and applicable specification/revision. Material certificates and additional testing are subject to mill capability and agreement.

No certificate or test is automatically included. Alloy designation alone does not establish drawing compliance; confirm specification, revision, temper, product form, dimensions and inspection requirements.

  • Mill chemistry and mechanical test results traceable to heat/cast and production lot.
  • Exact temper including T651 or T6511 stress-relief suffix; confirm any dimensional straightening requirements.
  • Specified tensile sampling orientation, thickness basis, elongation gauge length and dimensional tolerances.
  • AMS or ASTM compliance only when expressly ordered and demonstrated; commercial alloy designation alone is insufficient.
  • EN 10204 3.1 inspection certificate where agreed; special inspection, ultrasonic testing or aerospace release requirements by prior agreement.
  • Certificate of Conformity where agreed
  • Heat-treatment records and hardness testing where specified
  • Customer-specific chemical analysis, mechanical tests and ultrasonic inspection where applicable and agreed

Material enquiry

Request a material quotation

Aluminium Alloy 6061 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.