Representative extruded aluminium profiles and tubes

Materials Supply / Aluminium Alloys

Aluminium Alloy 6063

Heat-treatable Al–Mg–Si alloy for quality extruded profiles

6063 is a heat-treatable aluminium–magnesium–silicon alloy widely used for extruded architectural and engineering profiles, tubes and heat sinks. It is not primarily an aerospace plate alloy.

Strength depends on the product form, specification, temper and section size. The independently sourced North American and European tables are alternative procurement bases, not interchangeable datasets.

Illustrative aluminium materials and fabricated components, not certified alloy stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

Producer literature verifies standard and custom solid profiles, architectural shapes, heat sinks and seamless/structural tube and pipe. Geometry, size, condition and tolerances require mill confirmation; profile tables are not tube guarantees. No plate, forging or rolled-sheet supply is implied.

  • Extruded profiles and structural shapes
  • Seamless and structural tube and pipe

Material overview

Aluminium Alloy 6063

An extrusion-focused aluminium alloy combining good extrudability, surface finish, anodising response and corrosion resistance.

  • Magnesium and silicon enable precipitation strengthening through Mg–Si precipitates. Solution treatment and quenching retain solute for subsequent natural or artificial ageing; precipitate development changes strength and ductility.
  • T5 is cooled from an elevated-temperature shaping process and artificially aged. T6 is solution heat treated and artificially aged. A producer-qualified press-quench route can achieve certain solution-treated tempers, but this does not make T5 and T6 identical.
  • 6063 is selected for extrudability and visible surface quality. Specify alloy variant, surface preparation, finish and exposed-face requirements rather than assuming every extrusion is decorative-anodising quality.

Designations and procurement references

Designations and procurement references
Designation / referenceScope and qualification
AA 6063Registered wrought alloy; chemistry from AA Teal Sheets
EN AW-6063 [AlMg0.7Si]Hydro European extrusion designation
EN 573-3:2013Chemistry basis cited in Hydro European sheet; full standard not reviewed
EN 755-2:2016Mechanical-property basis cited by Hydro for extruded profiles
EN 515:1993Temper definition edition cited by Hydro; no claim of reviewing the licensed standard
ASTM / AMS / UNSNo unreviewed specification or equivalence asserted; confirm required product standard and revision on order

Designation identity does not establish interchangeability of product specifications or aerospace approval.

Specification review

Technical verification requirements

  • Designations / form / temper / dimensions

    Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.

    Obtain applicable controlled specification and producer confirmation; submit to technical review.

  • Mechanical conditions / gauge / orientation

    Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.

    Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.

Grade selection

6061, 6063 and 6082 compared

6061, 6063 and 6082 compared
Aspect606160636082
Registered Mg / Si, mass %Mg 0.8–1.2 / Si 0.40–0.8Mg 0.45–0.9 / Si 0.20–0.6Mg 0.6–1.2 / Si 0.7–1.3
Principal additional elementsCu 0.15–0.40%; Cr 0.04–0.35%; Mn ≤0.15%Cu, Cr and Mn each ≤0.10%Mn 0.40–1.0%; Cr ≤0.25%; Cu ≤0.10%
Metallurgical classificationPrecipitation-hardenable Al-Mg-Si-Cu-CrPrecipitation-hardenable Al-Mg-SiPrecipitation-hardenable Al-Mg-Si-Mn
Common temper distinctionsT4 natural ageing; T6 artificial ageing; T651/T6511 include specified stress reliefT5 cooling from shaping then artificial ageing; T6 separate solution heat treatment and artificial ageingT4/T6 and stress-relieved product conditions depend on mill and product specification
Strength selectionEngineering strength depends on form, section and temperOften selected for extrusion quality rather than maximum strengthStructural strength depends on form, section and temper; not universally stronger than 6061
Extrudability and surface finishStructural and precision extrusion productsGood extrudability and surface finish; anodising quality still requires surface/process controlStructural extrusions; surface expectations require mill confirmation
MachinabilityAged tempers suited to machining; stress-relieved stock can reduce movementSofter tempers require chip and finish controlAged structural products suited to machining; residual stress still matters
Welding and formingWelding can soften aged HAZ; softer conditions improve formingGood weldability; HAZ and joint strength are not parent T5/T6 strengthWelding can soften aged HAZ; qualify joint properties
Corrosion protectionGood general resistance, not universal seawater immunityOften selected for corrosion resistance and anodised finishGood general resistance; coastal suitability remains environment-specific
Typical product focusSheet/plate, bar and extrusions subject to ordered requirementsExtruded profiles, bar and tubeEuropean structural plate, bar and extrusions
Engineering usesMachined parts, fixtures and structural fittingsFrames, enclosures, profiles and finished extrusionsStructural and transport components and machined equipment
Specification substitutionCommercial designation is not aerospace AMS approvalExtrusion-specific requirements are not plate requirementsCannot automatically replace 6061 on an AMS-controlled drawing

Qualitative selection guide, using registered AA chemistry and the grade-specific producer references on these pages. No numerical strength ranking: temper, product form, section size and test basis are not matched. No alloy or temper is automatically interchangeable; confirm the drawing and ordered specification.

The Aluminum Association — Teal Sheets, December 2025; fabrication references on each grade page

Engineering reference

Technical data

Chemical composition limits — 6063 (AA)
ElementMass %Limit
Si0.20–0.6Range
Fe0.35Maximum
Cu0.10Maximum
Mn0.10Maximum
Mg0.45–0.9Range
Cr0.10Maximum
Zn0.10Maximum
Ti0.10Maximum
Other elements, each0.05Maximum
Other elements, total0.15Maximum
AlRemainderBalance

Registered AA limits, not nominal or certified heat analysis. Ranges show minimum–maximum; all other numeric entries are maxima. AA other-element provisions apply. EN requirements are not independently merged into this table; agree the governing chemistry standard and mill certificate. Separately registered suffix alloys are not included.

The Aluminum Association — Teal Sheets, December 2025

Typical physical properties
PropertyValueBasis
Density2.70 g/cm³Typical
Elastic modulus69 GPaTypical
Rigidity modulus26 GPaTypical
Melting range615–655 °CRange, not a treatment schedule
Specific heat capacity901 J/(kg·K)Typical
Linear expansion coefficient23.5 × 10⁻⁶ K⁻¹Typical
Thermal conductivity, T6201 W/(m·K)Typical
Electrical resistivity, T635 nΩ·mTypical

Hydro labels these typical properties at room temperature 20 °C, referencing MNC Handbok nr 12 (1989). Conductivity/resistivity explicitly T6; other cells are presented without a separate temper. Melting interval is not a test temperature.

T4 — EN extruded profile

6063-T4 — extruded profile (EN basis)
Wall thickness t (mm)Rp0.2 min (MPa)Rm min (MPa)A min (%)A50mm min (%)HBW typical
≤2565130141250

Producer reproduces EN 755-2:2016 values; standard itself not reviewed. Tensile test temperature not stated. HBW is informational, not an acceptance minimum. A and A50mm are separate elongation measures. For a mixed-thickness profile, Hydro states that the lowest specified value applies to the whole section. T4, T6, T64 and T66 properties may be obtained by press quenching.

T5 — EN extruded profile

6063-T5 — extruded profile (EN basis)
Wall thickness t (mm)Rp0.2 min (MPa)Rm min (MPa)A min (%)A50mm min (%)HBW typical
≤101301758665
>10–251101607565

Producer reproduces EN 755-2:2016 values; standard itself not reviewed. Tensile test temperature not stated. HBW is informational, not an acceptance minimum. A and A50mm are separate elongation measures. For a mixed-thickness profile, Hydro states that the lowest specified value applies to the whole section. T4, T6, T64 and T66 properties may be obtained by press quenching.

T6 — EN extruded profile

6063-T6 — extruded profile (EN basis)
Wall thickness t (mm)Rp0.2 min (MPa)Rm min (MPa)A min (%)A50mm min (%)HBW typical
≤101702158675
>10–251601958675

Producer reproduces EN 755-2:2016 values; standard itself not reviewed. Tensile test temperature not stated. HBW is informational, not an acceptance minimum. A and A50mm are separate elongation measures. For a mixed-thickness profile, Hydro states that the lowest specified value applies to the whole section. T4, T6, T64 and T66 properties may be obtained by press quenching.

T64 — EN extruded profile

6063-T64 — extruded profile (EN basis)
Wall thickness t (mm)Rp0.2 min (MPa)Rm min (MPa)A min (%)A50mm min (%)HBW typical
≤15120180121065

Producer reproduces EN 755-2:2016 values; standard itself not reviewed. Tensile test temperature not stated. HBW is informational, not an acceptance minimum. A and A50mm are separate elongation measures. For a mixed-thickness profile, Hydro states that the lowest specified value applies to the whole section. T4, T6, T64 and T66 properties may be obtained by press quenching.

T66 — EN extruded profile

6063-T66 — extruded profile (EN basis)
Wall thickness t (mm)Rp0.2 min (MPa)Rm min (MPa)A min (%)A50mm min (%)HBW typical
≤102002458680
>10–251802258680

Producer reproduces EN 755-2:2016 values; standard itself not reviewed. Tensile test temperature not stated. HBW is informational, not an acceptance minimum. A and A50mm are separate elongation measures. For a mixed-thickness profile, Hydro states that the lowest specified value applies to the whole section. T4, T6, T64 and T66 properties may be obtained by press quenching.

O — Hydro NA extrusion

6063-O — Hydro North America extrusion
Specimen section thickness (mm)Ultimate tensile strength (MPa)0.2% offset yield strength (MPa)Elongation min (%)
All130 maximumNot specified18

Mechanical test temperature not stated. Producer limits, not typical values; thickness is that of the section from which the tension specimen is taken. Source metric thickness bands retained without reconciling inch rounding. Elongation in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. T52 has both lower and upper strength limits; it is not interchangeable with T5.

T1 — Hydro NA extrusion

6063-T1 — Hydro North America extrusion
Specimen section thickness (mm)Ultimate tensile strength (MPa)0.2% offset yield strength (MPa)Elongation min (%)
≤12.50115 minimum60 minimum12
>12.50–25.00110 minimum55 minimum12

Mechanical test temperature not stated. Producer limits, not typical values; thickness is that of the section from which the tension specimen is taken. Source metric thickness bands retained without reconciling inch rounding. Elongation in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. T52 has both lower and upper strength limits; it is not interchangeable with T5.

T4 — Hydro NA extrusion

6063-T4 — Hydro North America extrusion
Specimen section thickness (mm)Ultimate tensile strength (MPa)0.2% offset yield strength (MPa)Elongation min (%)
≤12.50130 minimum70 minimum14
>12.50–25.00125 minimum60 minimum14

Mechanical test temperature not stated. Producer limits, not typical values; thickness is that of the section from which the tension specimen is taken. Source metric thickness bands retained without reconciling inch rounding. Elongation in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. T52 has both lower and upper strength limits; it is not interchangeable with T5.

T5 — Hydro NA extrusion

6063-T5 — Hydro North America extrusion
Specimen section thickness (mm)Ultimate tensile strength (MPa)0.2% offset yield strength (MPa)Elongation min (%)
≤12.50150 minimum110 minimum8
>12.50–25.00145 minimum105 minimum8

Mechanical test temperature not stated. Producer limits, not typical values; thickness is that of the section from which the tension specimen is taken. Source metric thickness bands retained without reconciling inch rounding. Elongation in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. T52 has both lower and upper strength limits; it is not interchangeable with T5.

T52 — Hydro NA extrusion

6063-T52 — Hydro North America extrusion
Specimen section thickness (mm)Ultimate tensile strength (MPa)0.2% offset yield strength (MPa)Elongation min (%)
≤25.00150–205 limits110–170 limits8

Mechanical test temperature not stated. Producer limits, not typical values; thickness is that of the section from which the tension specimen is taken. Source metric thickness bands retained without reconciling inch rounding. Elongation in 2 inches or 4D; not required where a standard specimen cannot be taken or for shapes thinner than 0.062 inch. T52 has both lower and upper strength limits; it is not interchangeable with T5.

Solution treatment, quenching and ageing

Solution treatment makes strengthening solute available; quenching retains a supersaturated condition, then natural ageing or artificial ageing develops Mg–Si precipitates. Section thickness and cooling history affect response and residual stress; use a qualified alloy- and product-specific procedure, not a generic numeric schedule.

O, T1 and T4

O is annealed to obtain the lowest-strength temper. T1 is cooled from elevated-temperature shaping and naturally aged; T4 is solution heat treated and naturally aged. Neither is equivalent to artificially aged T6.

T5 versus T6

T5 is cooled from an elevated-temperature shaping process and artificially aged; T6 is solution heat treated and artificially aged. Hydro notes that cold-work effects from straightening are not recognised in these standard temper properties. Use the table for the exact form, thickness and procurement basis.

T52 and T66: preserve the designation system

Hydro North America groups T52 with the T5 cooling/artificial-ageing family and publishes a bounded strength range. Its precise additional ANSI H35.1 definition was not obtained and is not inferred. Hydro Europe describes T66 under EN 515:1993 as solution heat treated and artificially aged with a mechanical-property level higher than T6 through special process control. This EN description is not presented as an independently verified ANSI definition.

T64 bending quality and stress relief

Hydro Europe identifies T64 as solution heat treated and artificially underaged to improve formability, and calls it bending quality. No 6063-T651 or T6511 product combination is offered here: stress-relief suffixes are not generic synonyms for T6, and must be verified for the specified alloy and product.

Conceptual description only, not an operating instruction. No invented furnace temperatures, hold times or quench schedule. Quenching can introduce residual stress and section-dependent distortion; verify tolerances after machining and welding.

Material selection

Corrosion resistance & performance

Hydro reports good general corrosion resistance and resistance to stress-corrosion cracking in heat-treated 6063. This is not immunity in every environment.

Avoid unprotected dissimilar-metal contacts that can drive galvanic attack. Select surface treatment and assembly details for the service exposure.

Pitting, intergranular attack and stress-corrosion suitability require exposure-, temper- and product-specific assessment. Anodising or conversion coatings and galvanic isolation should be selected for the actual environment; these pages give no universal seawater or corrosion-life guarantee.

Typical applications

Engineering applications

  • Architectural profiles, window and door frames
  • Railings and furniture profiles
  • Electrical components and conduit
  • Heat sinks
  • Irrigation pipe and tube
  • Custom solid profiles for general engineering

Subsequent manufacturing

Machining & processing

Extrusion and surface finish

Good extrudability supports complex constant-section shapes. Excellent anodising response is a selection advantage, not an automatic decorative-finish guarantee. Agree exposed faces, finish samples and protective packaging; Hydro notes that ink stencilling is normally avoided to protect appearance.

Forming and machining

Temper affects formability: Hydro specifies T64 bending quality and lists softer naturally aged conditions separately. Qualify bend radii and tooling for the actual profile. Hydro rates 6063 machinability below 6082; do not substitute a profile alloy for a machining alloy without review.

Welding and brazing

6063 can be welded and brazed by commercial processes. Heat from welding can reduce strength in the weld region of T6 material; parent-metal tensile minima are not guaranteed as-welded joint strengths. Select filler and a qualified weld procedure for the joint and service. No universal post-weld restoration schedule is specified.

Thermal exposure and dimensional control

Natural and artificial ageing, quench rate and section thickness affect precipitate development and residual stress. Prolonged heating may overage the material; no maximum service temperature or numerical high-temperature design allowable is asserted. Plan machining, clamping and welding sequences to control distortion; post-weld heat treatment must be qualified rather than assumed to restore parent strength.

Material certification & testing

Order by exact alloy, temper, product form, dimensions and specification revision, with the required inspection document agreed before supply.

No certificate or test is automatically included. Alloy designation alone does not establish drawing compliance; confirm specification, revision, temper, product form, dimensions and inspection requirements.

  • Request mill chemistry and mechanical test results linked to heat / cast / lot identification.
  • Agree EN 10204 3.1 documentation where contractually required and available; this is a purchase requirement, not an assertion of existing certification.
  • Specify surface finish, anodising requirements, dimensional tolerances, traceability marking and protective packaging.
  • State any aerospace or customer-specific approval explicitly; commercial 6063 is not automatically aerospace-qualified.
  • Certificate of Conformity where agreed
  • Heat-treatment records and hardness testing where specified
  • Customer-specific chemical analysis, mechanical tests and ultrasonic inspection where applicable and agreed

Material enquiry

Request a material quotation

Aluminium Alloy 6063 supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.