Representative precision cold-rolled iron-nickel alloy strip coils

Materials Supply / Controlled-Expansion & Electronic Alloys

Kovar (Fe–Ni–Co sealing alloy)

Fe–29Ni–17Co | UNS K94610 | EN 1.3981 | ASTM F15

Kovar is used where a metal must be sealed to hard glass or ceramic. Its expansion is low and nearly flat up to roughly 400–450°C, then rises above the Curie temperature.

It is not interchangeable with the Fe–Ni sealing alloys 42, 46, 48 or 52, which match different glasses.

Imagery is illustrative metal product forms, not certified Kovar stock or evidence of Quest stockholding.

Raw & semi-finished materials

Available material forms

Carpenter lists flat/round bar, billet, strip and wire; ASTM F15 covers wire, rod, bar, strip, sheet and tubing. Confirm forms, sizes and availability at enquiry.

  • Round and flat bar, billet
  • Strip and sheet
  • Wire
  • Tubing

Material overview

Kovar (Fe–Ni–Co sealing alloy)

An iron–nickel–cobalt alloy whose expansion is matched to hard borosilicate glasses and alumina ceramics for hermetic seals.

  • Carpenter publishes annealed mean CTE from 25°C to eleven upper temperatures; each value applies only to its own interval.
  • Seal success depends on hydrogen annealing/decarburising and controlled oxidation before sealing.

Designations and specifications

Designations and specifications
Designation / standardScope and qualification
UNSK94610 (ASTM F15, Carpenter)
EuropeanEN 1.3981 (VDM, Special Metals)
Producer namesCarTech Kovar; VDM Alloy 29-18 / Pernifer 2918; Special Metals NILO K; Aperam DILVER (product page lists K94100 — suspected listing error)
ASTM F15Iron–nickel–cobalt sealing alloy; wire, rod, bar, strip, sheet and tubing
AMS 7726Cited by Special Metals for NILO K wire; current revision not authenticated
MIL-I-23011 / AMS-I-23011Class mapping not verified

Obtain controlled current standards before ordering.

ASTM F15-04(2017) — official listing

Specification review

Technical verification requirements

  • Heat treatment

    Carpenter CTE conditioning wording ambiguous.

    Confirm conditioning cycle with the producer or ASTM F15 text.

  • Physical properties / chemistry

    Carpenter vs NILO K density and resistivity differ; Carpenter Mn/Si nominal vs maxima conflict; Aperam DILVER lists K94100.

    Use the certificate of the ordered heat.

  • Specifications

    AMS 7726 revision and MIL-I-23011 class mapping not verified.

    Obtain controlled current standards.

Grade selection

Controlled-expansion alloys — distinct grades, not substitutes

Controlled-expansion alloys — distinct grades, not substitutes
AlloyNominal base (mass %)UNS (as verified)Published mean CTE and intervalPrimary intended use (per source)
Invar 36Fe–36NiK93601 / K93603 (Carpenter)1.30 × 10⁻⁶/K to 93°C; lower reference not stated (Carpenter)Dimensionally stable structures, tooling, instruments
Super InvarFe–32Ni–5.5CoK93500 (Carpenter)0.63 × 10⁻⁶/K, −55 to 95°C (Carpenter)Lower expansion than Invar 36 over a narrow range
KovarFe–29Ni–17CoK94610 (ASTM F15)5.85 × 10⁻⁶/K, 25–100°C; 5.13 × 10⁻⁶/K, 25–300°C (Carpenter, annealed)Seals to hard borosilicate glass and alumina ceramics
Alloy 42Fe–41/42NiK94100 (Carpenter, VDM)5.40 × 10⁻⁶/K, 21–343°C (Carpenter); 5.3 × 10⁻⁶/K, 20–300°C (NILO 42)Glass sealing (e.g. 1075, 0120, 0010 glasses per Carpenter), lead frames
Alloy 46Fe–46Ni(–0.4Ti, Carpenter)Not verifiedNot verifiedEnamelled-resistor terminal bands (Carpenter)
Alloy 48Fe–48NiK94800 (Special Metals, Aperam)8.7 × 10⁻⁶/K, 20–300°C (NILO 48)Soft lead or soda-lime glass seals
Alloy 52Fe–51/52NiN14052 (Aperam, VDM)Not verified from a primary producer tableSoft-glass seals (Aperam)

Each value keeps its own producer, interval and conditioning; values from different sources are not directly comparable. Glass-to-metal sealing requires matching the alloy expansion curve to the specific glass or ceramic over the whole sealing-to-service temperature range — Kovar and Alloys 42/46/48/52 are not interchangeable.

Engineering reference

Technical data

Chemical composition — Carpenter
ElementMass %
Nickel29 (nominal)
Cobalt17 (nominal)
Manganese0.30
Silicon0.20
Carbon0.02 max
IronBalance

Carpenter historical datasheet gives Mn and Si as nominal; its current product page lists them as maxima — unresolved. Not ASTM F15 acceptance limits.

Physical properties and mean thermal expansion — Carpenter, annealed
Property / intervalProducer valueBasis
Density8.36 g/cm³ (0.3020 lb/in³)Temperature and condition not stated
Elastic modulus138 GPa (20.0 × 10³ ksi)Temperature and condition not stated
Electrical resistivity294 Ω·circ-mil/ft21°C (70°F)
Curie temperature435°C (815°F)—
Mean CTE 25–100°C5.85 × 10⁻⁶/K (3.25 × 10⁻⁶/°F)Annealed
Mean CTE 25–200°C5.20 × 10⁻⁶/K (2.89 × 10⁻⁶/°F)Annealed
Mean CTE 25–300°C5.13 × 10⁻⁶/K (2.85 × 10⁻⁶/°F)Annealed
Mean CTE 25–350°C4.90 × 10⁻⁶/K (2.72 × 10⁻⁶/°F)Annealed
Mean CTE 25–400°C5.06 × 10⁻⁶/K (2.81 × 10⁻⁶/°F)Annealed
Mean CTE 25–450°C5.26 × 10⁻⁶/K (2.92 × 10⁻⁶/°F)Annealed
Mean CTE 25–500°C6.14 × 10⁻⁶/K (3.41 × 10⁻⁶/°F)Annealed
Mean CTE 25–600°C7.81 × 10⁻⁶/K (4.34 × 10⁻⁶/°F)Annealed
Mean CTE 25–700°C9.11 × 10⁻⁶/K (5.06 × 10⁻⁶/°F)Annealed
Mean CTE 25–800°C10.31 × 10⁻⁶/K (5.73 × 10⁻⁶/°F)Annealed
Mean CTE 25–900°C11.25 × 10⁻⁶/K (6.25 × 10⁻⁶/°F)Annealed

Mean (secant) coefficients from 77°F (25°C); no instantaneous CTE table was verified. Metric values are converted from the published °F figures. Special Metals NILO K gives density 8.16 g/cm³ and resistivity 43 µΩ·cm at 20°C — kept separate, not merged.

Strip annealed 999°C 30 min, furnace cooled — Carpenter typical

Kovar — annealed strip, parallel to rolling
PropertyProducer typicalBasis
0.2% yield strength345 MPaTest temperature not stated
Ultimate tensile strength517 MPaTest temperature not stated
Elongation30%50.8 mm gauge
Hardness68 HRB—

Carpenter typical values for strip only, not specification limits.

Degas / anneal (Carpenter)

Degrease, then anneal in wet hydrogen at 838–1099°C (about 2 h at the low end to 20 min at the high end); cool in the same atmosphere below 299°C before removal. Avoid carbon pick-up.

Oxidation for hard-glass seals (Carpenter)

Oxidise in air at 650–700°C to a thin, adherent dark-grey to slightly brown film.

NILO K alternative (Special Metals)

Anneal 850–1000°C in hydrogen or cracked ammonia; decarburise in wet hydrogen 900–1050°C for 1 h; oxidise 600–1000°C depending on required oxide thickness.

CTE test conditioning

Carpenter’s CTE conditioning wording (900°C 1 h / 1099°C 15 min in hydrogen) is ambiguous in the source and is not presented as a certified cycle. No transformation reported after 4 h at −80°C.

Producer-specific alternatives, not interchangeable mandated cycles. No quantified before/after expansion effect is published.

Typical applications

Engineering applications

  • Hermetic glass-to-metal seals with hard borosilicate glass
  • Metal-to-ceramic seals with alumina (per Special Metals)
  • Electronic packages, headers and lead-throughs
  • Vacuum and microwave tube components

Subsequent manufacturing

Machining & processing

Machining and forming

Machining and cold forming introduce residual stress that changes expansion behaviour and dimensional stability; final stabilising or annealing treatments should follow rough machining, near final size.

Magnetic transformation

The low-expansion range of these Fe–Ni(–Co) alloys ends near their Curie (or inflection) temperature; above it, expansion rises sharply. Do not extrapolate a mean CTE beyond its stated interval.

Not a corrosion-resistant alloy

These alloys are not stainless; protection must be specified for humid or corrosive service.

Application evidence

Listed applications are producer-cited categories, not claims of stock or component approval.

Material certification & testing

Documentation must be agreed for the actual alloy, specification, product form, temper and any expansion-test requirement. Expansion acceptance depends on the specified interval and pre-test conditioning.

No certificate, expansion guarantee, sealing approval or alloy equivalence is automatic. Low-expansion and sealing alloys are not interchangeable; quotation controls remain disabled.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the producing mill
  • Chemical analysis to the ordered specification
  • Thermal-expansion test report over the specified interval and conditioning, only where ordered

Material enquiry

Request a material quotation

Kovar (Fe–Ni–Co sealing alloy) supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.