Representative ground nickel-based alloy round bars

Materials Supply / Nickel, Cobalt & High-Temperature Alloys

Alloy 800HT Nickel-Iron-Chromium Alloy

Austenitic Nickel-Iron-Chromium Alloy | UNS N08811 | W.Nr. 1.4959

Controlled-composition nickel-iron-chromium alloy with restricted carbon and aluminium-plus-titanium for elevated-temperature creep and rupture resistance.

Also known commercially as INCOLOY® alloy 800HT. INCOLOY and 800HT are trademarks of the Special Metals Corporation group of companies. Quest Engineering does not own these trademarks.

Alloy 800, 800H and 800HT are separate grades. Selection requires assessment of chemistry, grain size, treatment, product form and the applicable specification; no automatic substitution is implied.

Raw & semi-finished materials

Available material forms

Producer-listed potential forms only. Availability depends on specification, dimensions, condition and supplier confirmation; no stock or immediate availability is implied.

  • Round Bar
  • Plate
  • Sheet
  • Strip
  • Pipe
  • Tube
  • Wire
  • Forging Stock
  • Cut-to-Size Material

Material overview

Alloy 800HT Nickel-Iron-Chromium Alloy

Controlled-composition nickel-iron-chromium alloy with restricted carbon and aluminium-plus-titanium for elevated-temperature creep and rupture resistance.

  • Controlled-composition nickel-iron-chromium alloy with restricted carbon and aluminium-plus-titanium for elevated-temperature creep and rupture resistance.
  • Typical producer properties are not guaranteed minima or design allowables.
  • Confirm the service environment and ordered product specification before selection.

Material specifications & designations

Material specifications & designations
Designation / specificationProduct form / scopeNotes
UNSN08811Grade-specific identifier
W.Nr. / EN1.4959SMC-047 lists 1.4876, 1.4958 and 1.4959 collectively without a one-to-one mapping. VDM H/HP designation table supports 1.4958 for H and 1.4959 for HP/N08811; 1.4876 is also an H reference under EN 10095. Not universal equivalence.
Alternative commercial nameINCOLOY® alloy 800HTSpecial Metals trademark; not a separate generic specification
ASTM B408Hot-/cold-worked rod and barPublic B408-22 scope explicitly includes N08811
ASTM B409Rolled plate, sheet and stripPublic B409-01 scope includes N08811; historical reference. ASTM WK100195 proposes removal of N08800/N08810/N08811 from B409-22; verify current revision.
ASTM B407Cold-worked and hot-finished annealed seamless pipe and tubePublic B407-04 scope explicitly includes N08811
ASTM B564ForgingsProducer-listed; current grade/condition requirements need full-standard review
ASTM B163Seamless condenser and heat-exchanger tubesProducer-listed; not a general pipe specification
ASTM B514Welded pipeProducer-listed; verify ordered grade and condition
ASTM B515Welded tubeProducer-listed; verify ordered grade and condition
ASTM B366Wrought fittingsProducer-listed; verify exact grade and fitting requirements
ASME SB 408Rod and barProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 409Plate, sheet and stripProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 407Seamless pipe and tubeProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 564ForgingsProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 163Seamless condenser/heat-exchanger tubeProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 514Welded pipeProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 515Welded tubeProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.
ASME SB 366FittingsProducer-listed; verify adopted Code edition, grade, condition and design rules; ASTM and ASME revisions are not automatically identical.

Grade associations are producer-listed, not a claim of certification. Public ASTM abstracts verify selected scopes only. Full current ASTM/ASME/AMS standards were not accessible. General-requirement companions B829/B906/B775/B751 are not standalone grade specifications. No filler-metal specification is represented as parent metal. No AMS parent-metal specification is independently established for this grade here. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • Designations / ordered product condition

    N08811/800HT restrictive carbon and Al+Ti controls and high-temperature solution treatment need purchase-order verification; do not generalise 800H data as certified HT minima. Existing cautions do not prove conformity; no allegation that every listed scope is wrong. Obtain the ordered revision and map each cited specification to form, dimensions, manufacture, delivery condition and acceptance tests.

    Obtain licensed ordered editions and issue a material-specific form/condition/size compliance matrix; retain existing caveats pending approval.

Grade selection

Alloy 800, 800H and 800HT compared

Alloy 800, 800H and 800HT compared
RequirementAlloy 800 (N08800)Alloy 800H (N08810)Alloy 800HT (N08811)
C, mass %≤0.100.05–0.100.06–0.10
Al, mass %0.15–0.600.15–0.600.25–0.60
Ti, mass %0.15–0.600.15–0.600.25–0.60
Al+Ti, mass %0.30–1.200.30–1.200.85–1.20
Grain sizeNot specified in general comparisonASTM No. 5 or coarserASTM No. 5 or coarser
Solution annealOrdinary annealing; not the H/HT creep-strength treatmentProducer normally uses 1150–1200°C to develop coarse grain1149°C minimum stated; basic practice normally 1150–1200°C
Typical useHeat exchangers, process equipment, furnace fixturesLong-term elevated-temperature creep dutyMore restricted chemistry for elevated-temperature creep/rupture duty

SMC-047 pp. 1–2, 10. General producer requirements, not a transcription of every current product standard. Special-order chemistry/grain limits can differ. Dual/triple certification depends on actual chemistry, processing, testing and the ordered specification; chemistry overlap alone does not establish conformity or interchangeability.

Engineering reference

Technical data

Chemical composition
ElementMass %
Nickel30.0–35.0
Chromium19.0–23.0
Iron≥39.5
Carbon0.06–0.10
Aluminium0.25–0.60
Titanium0.25–0.60
Aluminium + titanium0.85–1.20

SMC-047 Table 1, general requirements, N08811 column only. This table does not publish Mn, Si, S, Cu or P limits; none have been imported from another grade or source. Obtain the full ordered specification and heat analysis.

Physical properties
PropertyValueTemperature / basis
Density7940 kg/m³Temperature not stated
Melting range1357–1385°CMelting interval
Specific heat460 J/(kg·K)0–100°C
Tensile modulus196.5 GPa20°C; dynamic method
Electrical resistivity0.989 µΩ·m20°C
Thermal conductivity11.5 W/(m·K)20°C
Thermal conductivity21.1 W/(m·K)600°C
Mean coefficient of thermal expansion14.4 × 10⁻⁶/K21–100°C
Mean coefficient of thermal expansion17.1 × 10⁻⁶/K21–600°C
Mean coefficient of thermal expansion18.0 × 10⁻⁶/K21–800°C

SMC-047 Tables 2–4 explicitly state no significant physical/thermal differences between 800H/800HT and 800. Typical informational values, not specification limits; other condition details are not supplied. Density converted from 7.94 g/cm³.

Annealed plate

Mechanical properties — Annealed plate
PropertyValueBasis
Ultimate tensile strength536 MPaSMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.
0.2% yield strength150 MPaSMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.
ElongationNot reportedSMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.
Hardness126 BHNSMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.
Reduction of areaNot reportedSMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.

Typical producer measurements, not specification minima. Do not combine properties from other specimens, forms or conditions. SMC-047 Table 5: 20.7 mm annealed plate at 27°C; source explicitly reports jointly for 800H/800HT, not separate heat-specific tests. Gauge length/orientation and exact annealing cycle not stated.

Suitability depends on loading, temperature, exposure duration, atmosphere and service life; no single maximum service-temperature rating is implied.

Elevated-temperature tensile — annealed plate, Alloy 800HT

Elevated-temperature tensile — annealed plate, Alloy 800HT
Temperature °CUTS MPaYield MPaElongation %
425465130Not reported
54043290Not reported
65037893Not reported
705329109Not reported
76023690Not reported

SMC-047 Table 5, annealed 20.7 mm plate; the producer jointly labels these data 800H/800HT. Elongation is not tabulated; no graph values have been estimated. Typical measurements, not design allowables; yield is 0.2% offset.

Parent-metal creep/rupture performance is presented graphically in the bulletin; no numerical stress–rupture table is transcribed without validated extraction. Weld-metal rupture tables are not parent-metal data. Controlled chemistry and coarse-grain annealing improve creep/rupture strength over standard 800; do not equate 800H and 800HT design stresses.

High-temperature solution anneal

Producer basic practice normally uses 1150–1200°C, with time adjusted for section and furnace to achieve ASTM No. 5 or coarser, avoiding excessive grain growth.

800HT minimum treatment

800HT requires 1149°C minimum heat treatment in the producer introduction; the basic-practice section rounds to 1150°C. Confirm ordered product requirements.

Cooling and post-fabrication treatment

After hot working, air cool or faster; rapid cooling through 540–760°C is important when sensitisation is a concern. Stress relief is not automatically equivalent to solution annealing; assess cold strain, component restraint and service conditions.

Producer guidance only, not a qualified shop schedule. Holding time, cooling, final grain size and verification require product-specific agreement; no precipitation-ageing condition is implied.

Material selection

Corrosion resistance & performance

Chromium contributes resistance to oxidation and nickel contributes resistance to carburisation and selected corrosive environments; performance depends on atmosphere, contaminants and thermal cycling.

Sensitisation and carbide precipitation can affect intergranular corrosion behaviour. Assess the final fabrication and thermal history for the actual aqueous or high-temperature duty.

Resistance to chloride stress-corrosion cracking is not immunity to pitting, crevice attack or every chloride environment. No universal corrosion approval is implied.

Typical applications

Engineering applications

  • Steam/hydrocarbon reformer catalyst and convection tubing
  • Petrochemical furnace pigtails and outlet manifolds
  • Ethylene convection and cracking tubes
  • Furnace radiant tubes, muffles, retorts and fixtures
  • Steam superheating tubing and high-temperature heat exchangers

Subsequent manufacturing

Machining & processing

Machinability and tooling

Use rigid setups, sharp tools, suitable coolant and sustained cuts. Producer guidance includes coated carbide and high-speed-steel tooling; select for interrupted cuts and actual condition. No universal cutting speed is specified.

Work hardening and forming

Austenitic material work-hardens during cold deformation. Allow for springback, tool loads and intermediate annealing. For H/HT creep duty, restore and verify the required grain structure after substantial fabrication strain.

Welding

Use a qualified procedure and service-appropriate filler. Clean joints and control heat input and interpass conditions. Weld-metal strength and corrosion behaviour require separate assessment; matching parent-metal chemistry is not proof of weld creep performance.

Distortion and residual stress

Plan weld sequence, restraint and machining allowances to manage distortion. Highly strained or restrained parts can crack during reheating; agree any post-fabrication treatment with the design authority.

Finishing

Remove oil, grease and contaminants before heating; use controlled low-sulfur heating practice. Qualify descaling/pickling for nickel alloys and avoid embedded ferrous contamination.

Inspection

Verify grade identity, dimensions, surface condition and heat-treatment traceability. Where specified, assess grain size, weld quality and NDT acceptance against the ordered form and standard.

Material certification & testing

Documentation and inspection options are subject to order agreement and supplier confirmation:

Conformity must be demonstrated against the ordered specification, revision, product form and condition. Tests and certificates are not automatic; no blanket aerospace or pressure-code approval is implied.

  • EN 10204 3.1 material certificates
  • Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical testing
  • Heat-treatment records
  • Hardness testing
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable
  • Additional aerospace or customer-specific inspection requirements

Material enquiry

Request a material quotation

Alloy 800HT Nickel-Iron-Chromium Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.