Materials Supply / Titanium & Titanium Alloys
Ti-5553 / Ti-5Al-5V-5Mo-3Cr Titanium Alloy
Quasi-beta high-strength titanium alloy | UNS not verified | STA and BASCA
Ti-5553 is identified in the Aubert & Duval heading as Ti-5Al-5Mo-5V-3Cr and described as a quasi-beta alloy for structural parts and landing gear. The same sheet’s composition block prints vanadium 2.00, conflicting with the heading’s 5V. The name is retained as the producer’s designation, not a verified chemical analysis or purchase limit; obtain corrected producer chemistry.
No UNS designation could be confirmed from an authoritative source; distributor sources quote conflicting numbers, so none is shown.
Imagery is illustrative only; it does not identify a certified grade, product condition or available stock.
Raw & semi-finished materials
Available material forms
The producer sheet does not identify product forms, dimensions or an applicable wrought specification. Forgings and round bar shown here are enquiry options only, not verified producer availability or qualification. Confirm form, route, section, governing specification and heat-treatment condition before quotation; no stockholding is implied.
- Forgings
- Round bar
Material overview
Ti-5553 / Ti-5Al-5V-5Mo-3Cr Titanium Alloy
High-strength beta-rich titanium alloy (Ti-5Al-5Mo-5V-3Cr) used for structural parts and landing gear, usually delivered heat treated.
- Aubert & Duval states the alloy is generally delivered in the heat-treated condition for high-strength applications, and gives typical properties for two routes: solution treated and aged (STA) and beta annealed, slow cooled and aged (BASCA).
- The producer lists BASCA UTS 1100 MPa, within the STA range 1050–1250 MPa, so these data do not establish universally lower BASCA tensile strength. BASCA yield strength is listed as 950 MPa versus STA 1000–1100 MPa, and fracture toughness as 70 versus 55 MPa√m. These are typical/average reference values without a matched product-form, section or orientation basis, not a general performance guarantee.
- Wrought composition limits and aerospace material specifications were not verified from producer or SAE sources, so no composition table or specification list is given.
Designations and product specifications
| Designation / standard | Scope / status |
|---|---|
| Common names | Ti-5553; Ti-5-5-5-3; Ti-5Al-5Mo-5V-3Cr |
| UNS | Not verified — conflicting numbers in distributor sources |
| AMS / customer specifications | Not verified. Wrought material is typically ordered to aerospace customer specifications; confirm the governing document at enquiry. |
An SAE AMS document for Ti-5553 powder for additive manufacturing is cited by third parties; it would not cover wrought bar or forgings and has not been verified here.
Specification review
Technical verification requirements
Specification revision / product-form acceptance
Producer and historical references support much of the page; they do not establish all current ordered editions, product-form scope, treatment, section limits and acceptance provisions. This is a verification dependency, not evidence that these references are wrong.
Obtain ordered editions and record form/condition/thickness/orientation/test-temperature coverage separately for every listed specification; retain historical-data caveats.
Producer evidence / chemistry
Original producer PDF internally conflicts: heading states 5V, composition block states V2.00. Page appropriately omits limits but does not expose this original-source conflict. This is an internal source conflict, not two independently verified sources and not a confirmed wrong website chemistry limit.
Obtain corrected signed producer chemistry/specification; do not adopt 2% V or invent wrought limits.
Physical / density
Converted density presumes g/cm³, but accessible producer sheet prints no unit. Plausibility is not verification.
Ask producer to confirm unit and temperature; identify conversion as inferred until confirmed.
Forms / mechanics / manufacturing
Both typical mechanical tables match producer numbers, but source gives no form/section/orientation, wrought standard or exact cycle; stated welding/machining precautions are general titanium practice, not Ti5553 qualification. BASCA UTS1100 lies inside STA1050–1250, so “lower strength” is not universally demonstrated.
Obtain wrought producer form-specific sheet, chemistry, governing customer specification, condition routes and fabrication approval. Qualify strength comparison.
Grade selection
Ti-10-2-3 compared with Ti-5553
| Property | Ti-10-2-3 | Ti-5553 |
|---|---|---|
| UNS | R56410 | Not verified from an authoritative source |
| Nominal composition | Ti-10V-2Fe-3Al | Ti-5Al-5Mo-5V-3Cr (producer heading; composition block conflicts: V 2.00) |
| Classification (producer) | Near-beta (TIMET) | Quasi-beta (Aubert & Duval) |
| Beta transus (producer) | 800°C | 860°C |
| Density (producer) | 4650 kg/m³ | 4.64 (unit and temperature not stated; no verified SI conversion) |
| Heat-treatment routes (producer) | Solution treat below beta transus, then age 482–593°C for 8 h | STA, or BASCA (beta anneal, slow cool and age) |
| Typical applications | Landing gear, fittings, fasteners, actuators, flap tracks, rotor heads (TIMET) | Structural parts and landing gear (Aubert & Duval) |
Qualitative and physical producer comparison only. The two producer documents give strength on different bases (Ti-10-2-3 AMS guaranteed minimums by section; Ti-5553 typical ranges without section size), so no numerical strength comparison is shown. The alloys are not interchangeable.
Engineering reference
Technical data
| Property | Value | Temperature / basis |
|---|---|---|
| Density | 4.64 (unit not stated) | Temperature not stated; SI conversion withheld pending producer confirmation |
| Beta transus | 860°C | Producer value |
Other physical properties were found only in distributor sources and are omitted.
Solution treated and aged (STA) — producer typical
| Property | Typical value |
|---|---|
| Ultimate tensile strength | 1050–1250 MPa |
| 0.2% yield strength | 1000–1100 MPa |
| Elongation (5d) | 5–12% |
| Fracture toughness K1c | 55 MPa√m |
Typical or average producer values at ambient temperature, not guaranteed minimums. Product form and section size not stated. Heat-treatment temperatures not given. Test orientation, exact heat-treatment cycle and governing wrought specification are not identified; do not transfer these values to a selected bar or forging without form-specific verification.
Beta annealed, slow cooled and aged (BASCA) — producer typical
| Property | Typical value |
|---|---|
| Ultimate tensile strength | 1100 MPa |
| 0.2% yield strength | 950 MPa |
| Elongation (5d) | 6% |
| Fracture toughness K1c | 70 MPa√m |
Typical or average producer values, not guaranteed minimums. Product form and section size not stated. Not interchangeable with STA values. Test orientation, exact heat-treatment cycle and governing wrought specification are not identified; do not transfer these values to a selected bar or forging without form-specific verification.
Solution treated and aged (STA)
Producer route for high strength. Temperatures and times are not published in the producer source; use the ordered specification.
Beta annealed, slow cooled and aged (BASCA)
Producer route giving higher typical fracture toughness. Temperatures, cooling rate and ageing are not published in the producer source.
Producer beta transus 860°C. No exact schedules are given because none were verified from producer or specification sources; Ti-10-2-3 schedules do not apply.
Material selection
Corrosion resistance & performance
No grade-specific corrosion data were found in the producer source. Assess the actual environment, galvanic coupling and hydrogen absorption.
Typical applications
Engineering applications
- Aerospace structural parts, where specified and approved
- Landing gear components
Subsequent manufacturing
Machining & processing
Welding
Shield the weld pool, trailing hot metal and root with inert gas (or weld in a chamber) to prevent oxygen, nitrogen and hydrogen pick-up. Qualify the procedure and any post-weld heat treatment for the ordered condition.
Machining
High-strength beta-rich titanium concentrates heat at the cutting edge and can gall. Use rigid set-ups, sharp tools, positive feed without rubbing and generous coolant. Qualify speeds and feeds for the actual condition; no universal cutting speed is given.
Inspection
Confirm heat-treatment route (STA or BASCA), section size, toughness and ultrasonic requirements from the governing specification.
Material certification & testing
Agree documentation and inspection at enquiry stage for the actual alloy, specification, form, section size and condition.
Not every test or certificate is automatically included. Aerospace use requires the applicable specification and documented acceptance; these records do not confer approval.
- EN 10204 3.1 material certificate, where agreed with the supplier
- Certificate of Conformity
- Heat / batch and forging traceability to the mill certificate
- Heat-treatment records identifying solution and ageing temperatures and section size
- Mechanical tests (and fracture toughness where specified) to the ordered specification
- Ultrasonic, PMI, aerospace-specific or customer-specific testing only where applicable and agreed
Material enquiry
Request a material quotation
Ti-5553 / Ti-5Al-5V-5Mo-3Cr Titanium Alloy supplied to your material form, dimensions and specification.