Ti-6246 / Ti-6Al-2Sn-4Zr-6Mo Titanium Alloy

High-strength alpha–beta titanium alloy | UNS R56260 | Duplex annealed and solution treated and aged

Ti-6246 is a high-strength alpha–beta titanium alloy containing nominally 6% aluminium, 2% tin, 4% zirconium and 6% molybdenum. Its higher molybdenum content than Ti-6242 increases beta stability and heat-treatment response.

TIMET identifies this alloy as TIMETAL® 6-2-4-6. TIMETAL® is a registered trademark of Titanium Metals Corporation.

Imagery is illustrative only; it does not identify a certified grade, product condition or available stock.

Raw & semi-finished materials

Available material forms

Bar, wire and forgings per the AMS 4981 title cited by TIMET; sheet data are shown in TIMET literature. Supply remains subject to ordered specification, dimensions and supplier confirmation; no Quest stockholding is implied.

  • Round bar
  • Billet
  • Wire
  • Forgings
  • Sheet

Material overview

Ti-6246 / Ti-6Al-2Sn-4Zr-6Mo Titanium Alloy

Alpha–beta titanium alloy that can be heat treated to higher strengths in larger sections than Ti-6Al-4V, used in intermediate compressor stages.

  • TIMET states Ti-6246 can be heat treated to higher strengths in greater section sizes than Ti-6Al-4V, and that its properties depend on thermomechanical history.
  • Alpha–beta forged material gives enhanced strength, ductility and low-cycle fatigue; beta-forged material gives the best combination of low-cycle fatigue and fatigue-crack-growth resistance (TIMET).
  • Heat treatment trades strength against ductility: TIMET data show over-ageing (STOA) lowers strength relative to STA. Ti-6242 schedules do not apply.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
UNSR56260
AMS 4981Bars, wire and forgings, solution and precipitation treated; TIMET cites revision C (1990). Current revision not accessed.
MIL-T-9047GHistorical/cancelled: MIL-T-9047G cancelled by Notice 3, 10 February 2005. TIMET quotations are historical reference data, not current procurement acceptance. The notice points to SAE-AMS-T-9047; verify subsequent supersession and the application-specific replacement before ordering.

Ti-6242 specifications do not cover Ti-6246. No European material number verified.

Specification review

Technical verification requirements

  • Specification revision / product-form acceptance

    Producer and historical references support much of the page; they do not establish all current ordered editions, product-form scope, treatment, section limits and acceptance provisions. This is a verification dependency, not evidence that these references are wrong.

    Obtain ordered editions and record form/condition/thickness/orientation/test-temperature coverage separately for every listed specification; retain historical-data caveats.

  • Designations / mechanical selector

    Cancellation is established by notice text, but page does not identify historical/cancelled procurement status prominently. Existing caveat avoids claiming current validity; this is missing status, not proof the historical numbers are wrong.

    Add cancelled/historical status in subsequent controlled correction; determine contractual revision and application-specific replacement, not blanket equivalence.

  • Chemistry / heat schedule

    Important controlled element missing; source anomaly cannot be corrected by assumption. Heat-treatment panel omits temperature while mechanical note prints480–675°C; exact applicable cycle needs verification.

    Get signed H limit and complete time/temperature/cooling cycle, reconcile Fahrenheit/Celsius, section and ordered AMS4981 treatment.

Grade selection

Ti-6242 compared with Ti-6246

Ti-6242 compared with Ti-6246
PropertyTi-6242Ti-6246
UNSNot verified for the silicon-bearing reference chemistry; confirm ordered specification and mill designationR56260
Nominal compositionTi-6Al-2Sn-4Zr-2Mo (+ Si)Ti-6Al-2Sn-4Zr-6Mo
Molybdenum, mass %1.80–2.205.50–6.50
Classification (TIMET)Near-alpha, elevated-temperature alloyAlpha–beta, high-strength intermediate-temperature alloy
Strengthening / heat treatmentAnnealed, duplex/triplex annealed or solution treated and stabilisedHeat treatable to higher strength in larger sections than Ti-6Al-4V (DA, STA, STOA)
Elevated temperatureProducer states long-term application up to 538°C; creep data publishedIntermediate-temperature alloy; creep compared graphically with Ti-6Al-4V
Typical applicationsGas turbine compressor blades, discs, impellers; afterburner and hot airframe sheetIntermediate compressor-stage discs and blades, seals, airframe parts

Qualitative producer comparison only; the two TIMET datasheets do not give tensile data on the same product form, section and heat treatment, so no numerical strength comparison is shown. The alloys are not interchangeable and are covered by different specifications.

Engineering reference

Technical data

Chemical composition — AMS 4981 (as tabulated by TIMET)
ElementMass %Limit
TiBalanceRemainder
Al5.50–6.50Range
Sn1.75–2.25Range
Zr3.50–4.50Range
Mo5.50–6.50Range
Fe0.15Maximum
O0.15Maximum
C0.04Maximum
N0.04Maximum
Residual elements, each0.10Maximum
Residual elements, total0.40Maximum

One basis: the AMS 4981 column of TIMET Table 1 (MIL-T-9047 zirconium range 3.6–4.4% differs and is not combined). The printed hydrogen limit (0.125%) is anomalous and is omitted pending producer confirmation; no corrected value is inferred; obtain the hydrogen limit from the ordered specification.

Physical properties — producer reference values
PropertyValueTemperature / basis
Density4640 kg/m³22°C
Beta transus935°CProducer value
Melting (liquidus)1595–1675°CProducer value
Thermal conductivity7.61 W/(m·K)20–25°C
Specific heat502 J/(kg·K)Temperature not stated
Electrical resistivity1.90–2.05 µΩ·m20–25°C
Mean thermal expansion9.0 × 10⁻⁶ K⁻¹20–100°C
Young’s modulus107 GPa315°C
Young’s modulus100 GPa425°C

Producer values, not acceptance limits. Resistivity converted from the printed 75–80.7 µΩ·in (the printed SI figure is a misprint). Room-temperature modulus range (70–114 GPa) depends on texture and heat treatment.

Duplex annealed — historical bar reference (cancelled MIL-T-9047G)

Duplex annealed bar — room-temperature minimums
SectionUTS min0.2% YS minElongation minRA min
< 50.8 mm (2.00 in)1103 MPa1034 MPa10%25%
50.8–101.6 mm1034 MPa965 MPa8% (6% ST > 76 mm)20% (15% ST > 76 mm)

Historical reference only: MIL-T-9047G is cancelled (Notice 3, 10 February 2005). These quoted values are not current procurement acceptance limits; confirm the ordered replacement specification, form, condition, section and tests. As quoted by TIMET at 20°C. Duplex anneal: 870–900°C/1 h/AC + 540–593°C/8 h/AC. Properties apply in any grain direction unless noted.

Solution treated and aged — historical bar reference (cancelled MIL-T-9047G)

Solution treated and aged bar — room-temperature minimums
SectionUTS min0.2% YS minElongation minRA min
< 63.5 mm (2.50 in)1172 MPa1103 MPa10%20%
63.5–76.2 mm1138 MPa1068 MPa8%15%
76.2–101.6 mm1103 MPa1034 MPa8% (6% ST)15% (12% ST)

Historical reference only: MIL-T-9047G is cancelled (Notice 3, 10 February 2005). These quoted values are not current procurement acceptance limits; confirm the ordered replacement specification, form, condition, section and tests. As quoted by TIMET at 20°C. STA: 870–925°C/2–90 min/WQ or AC + 480–675°C/4–8 h (temperature range as printed). Not applicable to duplex-annealed material.

TIMET publishes elevated-temperature tensile strength for triplex-annealed sheet and a 0.2% creep comparison with Ti-6Al-4V as graphs only.

No numerical elevated-temperature or creep table is given, so none is shown and graph values are not read off. No maximum service temperature is stated.

Duplex anneal

870–900°C (1600–1650°F) for 1 hour, air cool; then 540–593°C (1000–1100°F) for 8 hours, air cool.

Solution treatment and ageing

Solution treat 870–925°C (1600–1700°F) for 2–90 minutes, water quench or air cool; age 4–8 hours (producer range as printed).

Example STA and STOA cycles

STA: 885°C/1 h/AC + 595°C/8 h/AC. STOA: 885°C/1 h/AC + 705°C/1 h/AC. Over-ageing lowers strength relative to STA in TIMET data.

TIMET producer schedules specific to Ti-6246, not copied from Ti-6242. Beta transus 935°C (producer). Microstructure (primary alpha content and morphology) strongly affects strength, ductility and fatigue.

Material selection

Corrosion resistance & performance

Producer literature used here does not provide grade-specific corrosion data. Assess the actual environment, including hydrogen absorption and galvanic coupling.

Typical applications

Engineering applications

  • Intermediate compressor-stage discs and blades, where specified and approved
  • Turbine engine seals
  • Airframe parts
  • High-strength aerospace forgings to the applicable specification

Subsequent manufacturing

Machining & processing

Forging

TIMET states forgeability and crack sensitivity similar to Ti-6Al-4V; alpha–beta and beta forging give different property balances.

Welding

Shield the weld pool, trailing hot metal and root with inert gas (or weld in a chamber) to prevent oxygen, nitrogen and hydrogen pick-up. Use clean preparation and qualified procedures; assess discoloured welds against the ordered acceptance criteria. Confirm weldability and post-weld treatment for the ordered condition.

Machining

Titanium concentrates heat at the cutting edge and can gall. Use rigid set-ups, sharp tools, positive feed without rubbing and generous coolant. Qualify speeds and feeds for the actual alloy and condition; no universal cutting speed is given. High-strength STA material is more demanding than annealed material.

Material certification & testing

Agree documentation and inspection at enquiry stage for the actual alloy, specification, form and condition.

Not every test or certificate is automatically included. PMI alone does not establish interstitial chemistry or grade conformity. Aerospace or medical use requires the applicable specification and documented acceptance; these records do not confer approval.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the mill certificate
  • Heat-treatment condition, mechanical test results and product-form traceability to the ordered specification
  • Mechanical tests and heat-treatment records to the ordered specification
  • Hardness, PMI, ultrasonic, aerospace-specific or customer-specific testing only where applicable and agreed

Material enquiry

Request a material quotation

Ti-6246 / Ti-6Al-2Sn-4Zr-6Mo Titanium Alloy supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.