Representative pickled titanium sheets

Materials Supply / Titanium & Titanium Alloys

Titanium Grade 12 / Ti-0.3Mo-0.8Ni

Lean near-alpha corrosion-resistant titanium alloy | UNS R53400 | Annealed

Grade 12 is a corrosion-resistant titanium alloy containing nominally 0.3% molybdenum and 0.8% nickel, used where enhanced corrosion resistance and useful mechanical strength are required.

TIMET describes TIMETAL® Grade 12 (also known as Code 12) as a lean, highly weldable near-alpha alloy. TIMETAL® is a registered trademark of Titanium Metals Corporation.

Imagery is illustrative only; it does not identify a certified grade, product condition or available stock.

Raw & semi-finished materials

Available material forms

Form/specification coverage from TIMET handbook Table 2 (B265, B337, B338, B348, B363 fittings, B381 forgings). Supply remains subject to ordered specification, dimensions and supplier confirmation; no Quest stockholding is implied.

  • Sheet
  • Strip
  • Plate
  • Bar and billet
  • Welded tube
  • Welded pipe
  • Forgings

Material overview

Titanium Grade 12 / Ti-0.3Mo-0.8Ni

Corrosion-resistant titanium alloy with nominally 0.3% molybdenum and 0.8% nickel, offering higher strength than Grade 2 and improved crevice-corrosion resistance.

  • TIMET states Grade 12 has higher strength than Grade 2 or Grade 7 at room and elevated temperatures, which can allow thinner sections, and is approved by the ASME Boiler Code for use up to 600°F (316°C) — a Code statement, not a general service limit.
  • Its microstructure and heat-treatment response differ from Grade 5; it is not strengthened by solution treatment and ageing.
  • Grade 12 mechanical properties are its own specification values and are not copied from Grade 2.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
UNSR53400
ASTM B265Grade 12; strip, sheet and plate; B265-20a basis.
ASTM B338Welded tubing (TIMET handbook Table 2); current revision unverified.
ASTM B337Welded pipe in TIMET handbook; current pipe standards B861/B862 coverage to be confirmed.
ASTM B348Bars and billets (TIMET handbook Table 2).
ASTM B381Grade F-12 forgings (TIMET handbook Table 2).
ASME SB-265, SB-338, SB-348, SB-381ASME Section II reproductions listed in TIMET handbook; confirm Code edition.

No AMS specification or European material number verified for Grade 12; none asserted.

Specification review

Technical verification requirements

  • Specification revision / product-form acceptance

    Producer and historical references support much of the page; they do not establish all current ordered editions, product-form scope, treatment, section limits and acceptance provisions. This is a verification dependency, not evidence that these references are wrong.

    Obtain ordered editions and record form/condition/thickness/orientation/test-temperature coverage separately for every listed specification; retain historical-data caveats.

Grade selection

Titanium Grades 5, 7, 9 and 12 compared

Titanium Grades 5, 7, 9 and 12 compared
PropertyGrade 5Grade 7Grade 9Grade 12
UNSR56400R52400R56320R53400
Nominal alloyingTi-6Al-4VTi-0.12–0.25PdTi-3Al-2.5VTi-0.3Mo-0.8Ni
Metallurgical classificationAlpha–beta alloyPalladium-modified commercially pure (alpha) titaniumAlpha–beta alloyLean near-alpha alloy (TIMET description)
Tensile strength, min MPa895345620483
0.2% yield strength, min MPa828275483345
Elongation in 50 mm, min %10201518
Relative formabilityLowest of the four at room temperatureHigh (similar to Grade 2)Intermediate; cold formableGood
Corrosion emphasisSeawater and general corrosionReducing acids and crevice conditions where Pd benefit is establishedClose to CP titaniumCrevice corrosion in hot brines; improved acid resistance over unalloyed grades
Typical applicationsAerospace structures, fasteners, engine and high-performance componentsChemical-process equipment, heat exchangers, pipingAerospace hydraulic tubing, honeycomb, pressure pipingChemical-process and brine heat exchangers, vessels, piping

Numerical rows are ASTM B265-20a annealed strip, sheet and plate minimums only; they are not typical values and must not be applied to bar, tube, forgings or heat-treated conditions. Qualitative rows come from TIMET producer literature. The grades are not interchangeable; select against the ordered specification and the actual service duty.

Engineering reference

Technical data

Chemical composition — ASTM B265 Grade 12
ElementMass %Limit
TiBalanceRemainder
Mo0.2–0.4Range
Ni0.6–0.9Range
Fe0.30Maximum
O0.25Maximum
C0.08Maximum
N0.03Maximum
H0.015Maximum
Residual elements, each0.10Maximum
Residual elements, total0.40Maximum

Single specification basis: ASTM B265-20a heat-analysis limits for strip, sheet and plate, reproduced through ASME SB-265. These are specification limits, not nominal values and not certified analysis. Other product-form specifications (bar, tube, pipe, forgings, AMS) can carry different hydrogen or interstitial limits; check the ordered specification. Product-analysis tolerances are separate. TIMET quotes nominal Mo 0.3%, Ni 0.8%; nominal values are not certified limits.

Physical properties — producer reference values
PropertyValueTemperature / basis
Density4510 kg/m³Temperature not stated
Tensile modulus103 GPaTemperature not stated
Torsional modulus42.7 GPaTemperature not stated
Specific heat544 J/(kg·K)24°C
Thermal conductivity19.0 W/(m·K)24°C
Electrical resistivity0.52 µΩ·m24°C
Thermal expansion9.54 × 10⁻⁶ K⁻¹24°C

Producer reference values, not acceptance limits. Melting range not given in this source and omitted.

Annealed — ASTM B265 sheet/plate minimum

Annealed sheet and plate — room-temperature minimums
PropertyRequirement
Ultimate tensile strength, minimum483 MPa
0.2% yield strength, minimum345 MPa
Elongation, minimum18% in 50 mm

B265 specification minimums, longitudinal and transverse; no maximum yield specified. TIMET quotes the same minimums for all product forms, with 25% reduction of area for bar, billet and forgings. Hardness not specified.

Stress relieving

TIMET handbook typical range: 480–650°C (900–1200°F) for ½–4 hours, air cool.

Annealing

TIMET handbook typical range: 650–760°C (1200–1400°F) for ½–4 hours, air cool.

Producer typical ranges; no solution treatment or ageing schedule applies. Clean before heating and avoid hydrogen-bearing atmospheres.

Material selection

Corrosion resistance & performance

TIMET reports significant improvement over unalloyed titanium in crevice corrosion in hot brines, and improved resistance to acids over unalloyed grades, with resistance under oxidising to mildly reducing conditions, especially chlorides.

TIMET data show Grade 12 and Grade 7 differ by environment (for example in boiling organic acids); neither is universally superior. Hot reducing acids, fluorides and high temperatures require specific test data.

Elevated-temperature aqueous corrosion resistance is separate from high-temperature structural strength. Assess galvanic coupling and hydrogen absorption.

Typical applications

Engineering applications

  • Chemical-process equipment in chloride and brine service, subject to assessment
  • Heat exchangers
  • Pressure vessels to applicable ASME/ASTM specifications
  • Industrial piping
  • Energy-sector equipment
  • Corrosion-resistant fabricated components

Subsequent manufacturing

Machining & processing

Forming

TIMET handbook gives minimum bend radii of 4T (under 1.8 mm) and 5T (1.8–4.75 mm) at room temperature; TIMET datasheet lists tube flattening and flaring capabilities.

Welding

TIMET describes Grade 12 as highly weldable. Use clean, dedicated preparation and qualified procedures. Shield the weld pool, trailing hot metal and root with inert gas (or weld in a chamber) to prevent oxygen, nitrogen and hydrogen pick-up; discoloured or contaminated welds require assessment against the ordered acceptance criteria.

Machining

Titanium has low thermal conductivity, concentrates heat at the cutting edge and can gall. Use rigid set-ups, sharp tools, positive feed without rubbing and generous coolant. Qualify speeds and feeds for the actual grade and condition; no universal cutting speed is given.

Inspection

Verify molybdenum and nickel on the certificate along with interstitial elements.

Material certification & testing

Agree documentation and inspection at enquiry stage for the actual grade, specification, form and condition.

Not every test or certificate is automatically included. PMI alone does not establish interstitial chemistry or grade conformity. Aerospace or pressure-equipment use requires the applicable specification and documented acceptance; these records do not confer approval.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the mill certificate
  • Chemical analysis identifying molybdenum (0.2–0.4%), nickel (0.6–0.9%) and interstitial elements
  • Mechanical tests and heat-treatment records to the ordered specification
  • Hardness, PMI, ultrasonic or additional aerospace inspection only where applicable and agreed

Material enquiry

Request a material quotation

Titanium Grade 12 / Ti-0.3Mo-0.8Ni supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.