Representative pickled titanium sheets

Materials Supply / Titanium & Titanium Alloys

Titanium Grade 7 / Ti-0.2Pd

Palladium-modified commercially pure titanium | UNS R52400 | Annealed

Grade 7 is commercially pure titanium modified with 0.12–0.25% palladium. It is not an alpha–beta alloy; it is listed in this combined catalogue group for convenience only.

TIMET identifies TIMETAL® 50A .15Pd with ASTM Grade 7. TIMETAL® is a registered trademark of Titanium Metals Corporation.

Imagery is illustrative only; it does not identify a certified grade, product condition or available stock.

Raw & semi-finished materials

Available material forms

Form/specification coverage from TIMET handbook Table 2 (B265, B337, B338, B348, B363 fittings, B367 castings, B381 forgings). Supply remains subject to ordered specification, dimensions and supplier confirmation; no Quest stockholding is implied.

  • Sheet
  • Strip
  • Plate
  • Bar and billet
  • Welded tube
  • Welded pipe
  • Forgings

Material overview

Titanium Grade 7 / Ti-0.2Pd

Commercially pure titanium with a small palladium addition (0.12–0.25%) for improved corrosion resistance in certain reducing and crevice environments.

  • Grade 7 has the same interstitial limits and tensile requirements as Grade 2 in ASTM B265, plus a palladium addition. TIMET notes the only difference of note is the improved corrosion resistance of the Pd-modified grades.
  • Grade 7 and Grade 2 are not automatically interchangeable: certificates must show Grade 7 palladium chemistry, and the corrosion benefit applies only in environments where it has been established.
  • Grade 7 is not precipitation hardened; no solution-treated-and-aged condition exists. ASTM B265 also lists Grade 7H, with a higher 400 MPa minimum tensile strength, intended primarily for pressure vessels.

Designations and product specifications

Designations and product specifications
Designation / standardScope / status
UNSR52400
ASTM B265Grades 7 and 7H; strip, sheet and plate; B265-20a basis.
ASTM B338Welded tubing (TIMET handbook Table 2); current revision unverified.
ASTM B337Welded pipe in TIMET handbook; pipe now generally ordered to B861 (seamless) / B862 (welded) — Grade 7 coverage to be confirmed.
ASTM B348Bars and billets (TIMET handbook Table 2).
ASTM B381Grade F-7 forgings (TIMET handbook Table 2).
ASME SB-265, SB-338, SB-348, SB-381ASME Section II reproductions listed in TIMET handbook; confirm Code edition.

No AMS specification or European material number verified for Grade 7; none asserted.

Specification review

Technical verification requirements

  • Specification revision / product-form acceptance

    Producer and historical references support much of the page; they do not establish all current ordered editions, product-form scope, treatment, section limits and acceptance provisions. This is a verification dependency, not evidence that these references are wrong.

    Obtain ordered editions and record form/condition/thickness/orientation/test-temperature coverage separately for every listed specification; retain historical-data caveats.

Grade selection

Titanium Grades 5, 7, 9 and 12 compared

Titanium Grades 5, 7, 9 and 12 compared
PropertyGrade 5Grade 7Grade 9Grade 12
UNSR56400R52400R56320R53400
Nominal alloyingTi-6Al-4VTi-0.12–0.25PdTi-3Al-2.5VTi-0.3Mo-0.8Ni
Metallurgical classificationAlpha–beta alloyPalladium-modified commercially pure (alpha) titaniumAlpha–beta alloyLean near-alpha alloy (TIMET description)
Tensile strength, min MPa895345620483
0.2% yield strength, min MPa828275483345
Elongation in 50 mm, min %10201518
Relative formabilityLowest of the four at room temperatureHigh (similar to Grade 2)Intermediate; cold formableGood
Corrosion emphasisSeawater and general corrosionReducing acids and crevice conditions where Pd benefit is establishedClose to CP titaniumCrevice corrosion in hot brines; improved acid resistance over unalloyed grades
Typical applicationsAerospace structures, fasteners, engine and high-performance componentsChemical-process equipment, heat exchangers, pipingAerospace hydraulic tubing, honeycomb, pressure pipingChemical-process and brine heat exchangers, vessels, piping

Numerical rows are ASTM B265-20a annealed strip, sheet and plate minimums only; they are not typical values and must not be applied to bar, tube, forgings or heat-treated conditions. Qualitative rows come from TIMET producer literature. The grades are not interchangeable; select against the ordered specification and the actual service duty.

Engineering reference

Technical data

Chemical composition — ASTM B265 Grade 7
ElementMass %Limit
TiBalanceRemainder
Pd0.12–0.25Range
Fe0.30Maximum
O0.25Maximum
C0.08Maximum
N0.03Maximum
H0.015Maximum
Residual elements, each0.10Maximum
Residual elements, total0.40Maximum

Single specification basis: ASTM B265-20a heat-analysis limits for strip, sheet and plate, reproduced through ASME SB-265. These are specification limits, not nominal values and not certified analysis. Other product-form specifications (bar, tube, pipe, forgings, AMS) can carry different hydrogen or interstitial limits; check the ordered specification. Product-analysis tolerances are separate.

Annealed — ASTM B265 sheet/plate minimum

Annealed sheet and plate — room-temperature specification limits
PropertyRequirement
Ultimate tensile strength, minimum345 MPa
0.2% yield strength, minimum275 MPa
0.2% yield strength, maximum450 MPa
Elongation, minimum20% in 50 mm

Specification limits for annealed Grade 7 sheet/plate, longitudinal and transverse; not typical values. Grade 7H requires 400 MPa minimum tensile strength with the same yield and elongation. Hardness and reduction of area not specified. Do not apply to bar, tube or forgings.

Stress relieving

TIMET handbook typical range: 480–595°C (900–1100°F) for ½–4 hours, air cool.

Annealing

TIMET handbook typical range: 650–760°C (1200–1400°F) for ½–4 hours, air cool.

Independent producer treatments for commercially pure and Pd grades, not a cumulative cycle. No solution treatment or ageing applies. Clean before heating and avoid hydrogen-bearing atmospheres.

Material selection

Corrosion resistance & performance

Palladium promotes repassivation of the protective oxide film and extends resistance into mildly reducing acids and hot chloride crevice conditions where unalloyed titanium may be attacked. TIMET handbook data compare Pd grades with unalloyed titanium in hydrochloric and other reducing media.

Grade 7 is not resistant to all acids. Resistance depends on acid type, concentration, temperature, aeration and oxidising species; hot concentrated reducing acids, fluorides and some dry or anhydrous media can still cause attack.

Assess crevice geometry, galvanic coupling and cathodic conditions, which can cause hydrogen absorption. Test or obtain specific data for the actual duty.

Typical applications

Engineering applications

  • Chemical-process equipment in reducing or fluctuating environments, subject to assessment
  • Heat exchangers and condensers
  • Pressure equipment to applicable ASME/ASTM product specifications
  • Corrosion-resistant piping and fittings
  • Marine and brine-handling equipment

Subsequent manufacturing

Machining & processing

Forming

TIMET handbook gives minimum bend radii of 4T (under 1.8 mm) and 5T (1.8–4.75 mm) for TIMETAL 50A .15Pd at room temperature. Forming behaviour is similar to Grade 2.

Welding

Use clean, dedicated preparation and qualified procedures. Shield the weld pool, trailing hot metal and root with inert gas (or weld in a chamber) to prevent oxygen, nitrogen and hydrogen pick-up; discoloured or contaminated welds require assessment against the ordered acceptance criteria. TIMET lists ERTi-0.2Pd filler (Pd 0.12–0.25%) for Grade 7; use matching filler so the weld retains the palladium benefit.

Machining

Titanium has low thermal conductivity, concentrates heat at the cutting edge and can gall. Use rigid set-ups, sharp tools, positive feed without rubbing and generous coolant. Qualify speeds and feeds for the actual grade and condition; no universal cutting speed is given.

Inspection

Verify palladium content on the certificate; PMI alone may not resolve Pd at these levels reliably.

Material certification & testing

Agree documentation and inspection at enquiry stage for the actual grade, specification, form and condition.

Not every test or certificate is automatically included. PMI alone does not establish interstitial chemistry or grade conformity. Aerospace or pressure-equipment use requires the applicable specification and documented acceptance; these records do not confer approval.

  • EN 10204 3.1 material certificate, where agreed with the supplier
  • Certificate of Conformity
  • Heat / batch traceability to the mill certificate
  • Chemical analysis identifying palladium (0.12–0.25%) and interstitial elements
  • Mechanical tests and heat-treatment records to the ordered specification
  • Hardness, PMI, ultrasonic or additional aerospace inspection only where applicable and agreed

Material enquiry

Request a material quotation

Titanium Grade 7 / Ti-0.2Pd supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.