Materials Supply / Aluminium Alloys
Aluminium Alloy 7075
High-strength aluminium–zinc–magnesium–copper aerospace alloy
High-strength aluminium–zinc–magnesium–copper aerospace alloy. Strength is developed by precipitation hardening, not by alloy designation alone.
7475 is not simply interchangeable 7075: tighter iron and silicon limits and controlled processing support improved fracture toughness and damage tolerance. Fatigue initiation strength and fatigue crack growth are separate design considerations.
Illustrative aluminium materials and engineered components, not certified alloy stock or evidence of Quest stockholding.
Raw & semi-finished materials
Available material forms
Producer-documented forms, not a stock or current availability commitment. Exact size, surface and temper require enquiry.
- Plate
- Bare sheet
- Alclad sheet
Material overview
Aluminium Alloy 7075
High-strength aluminium–zinc–magnesium–copper aerospace alloy. Temper, section size and orientation govern structural suitability.
- Zinc and magnesium provide the principal precipitation-hardening system; copper contributes to the high-strength response. Chromium influences grain structure and corrosion response. These are chromium-bearing alloys; no zirconium addition is inferred.
- Peak-aged and overaged conditions are not interchangeable. Strength, toughness, SCC, exfoliation resistance, fatigue response and machining stability must be balanced for the actual loading direction and section.
- Solution treatment and quenching establish a supersaturated condition for subsequent ageing. Quench rate varies through thick sections; residual stresses and through-thickness properties require attention. Stretch stress relief reduces, but does not eliminate, machining distortion.
Identification and specification basis
| Item | Basis |
|---|---|
| Alloy | 7075; wrought Al–Zn–Mg–Cu–Cr |
| Procurement | Specify product, temper, dimensions, orientation and applicable specification revision; no blanket equivalents asserted. |
| Historical producer references | Alcoa leaflet lists historical QQ-A-250 procurement references; not represented here as current approved purchasing specifications. |
Current licensed standards have not been reviewed. Historical references are not claims of present compliance or revision currency.
Specification review
Technical verification requirements
Designations / form / temper / dimensions
Product scopes were reviewed row by row. Recorded cross-references do not establish every current revision, ordered form, temper and dimensional limit; EN/UNS registries and complete controlled AMS/ASTM/EN texts were not inspected.
Obtain applicable controlled specification and producer confirmation; submit to technical review.
Mechanical conditions / gauge / orientation
Every selector/table was read. Typical, supplier minima and producer limits must remain distinct. Resolve missing orientation, specimen/gauge length, temperature, exact boundary inclusivity and test basis in the quoted notes; do not extend a specimen diameter to stock thickness or to other forms.
Produce a condition-by-condition acceptance matrix with form, thickness interval, tensile orientation, elongation basis, test temperature and source revision; omit unavailable values rather than infer them.
Toughness / thickness / corrosion
Retain exact form/temper/bare-versus-Alclad distinctions; historical producer data are not all current product guarantees. Verify toughness test validity and SCC acceptance by orientation.
Obtain applicable controlled specification and producer confirmation; submit to technical review.
Grade selection
7075 compared with 7020 and 7475
| Aspect | 7020 | 7075 | 7475 |
|---|---|---|---|
| Registered Cu mass % | ≤0.20 | 1.2–2.0 | 1.2–1.9 |
| Fe / Si maxima mass % | 0.40 / 0.35 | 0.50 / 0.40 | 0.12 / 0.10 |
| Alloy selection | Low-Cu weldable structural Al-Zn-Mg | High-strength aerospace Al-Zn-Mg-Cu | Controlled-impurity, toughness-oriented Al-Zn-Mg-Cu |
| Fusion welding | Producer-supported structural applications; qualify HAZ and joint strength | Not readily fusion-weldable for structural duty | Not readily fusion-weldable for structural duty |
| Damage tolerance | No numerical toughness equivalence asserted | Not inferred from tensile strength; method/temper/thickness/orientation control | Controlled impurities and producer processing support toughness selection; confirm the actual product |
| Temper and corrosion | Environment and welded condition must be assessed | Peak-aged vs overaged balance; SCC/exfoliation depend on stress and exposure | Plate and sheet temper/test routes differ; no corrosion immunity |
| Engineering uses | Loaded welded transport and construction structures | Specified structural fittings and high-strength machined parts | Drawing-approved fracture-critical skins, spars and bulkheads |
Qualitative engineering selection only; numeric chemistry is registered mass %. No numerical strength or toughness comparison is made because product form, temper, thickness, orientation and test basis are not matched. Neither material is universally superior or automatically interchangeable on a drawing.
The Aluminum Association — Teal Sheets, December 2025; grade-specific producer references below
Engineering reference
Technical data
| Element | Mass % | Limit |
|---|---|---|
| Si | 0.40 | Maximum |
| Fe | 0.50 | Maximum |
| Cu | 1.2–2.0 | Range |
| Mn | 0.30 | Maximum |
| Mg | 2.1–2.9 | Range |
| Cr | 0.18–0.28 | Range |
| Zn | 5.1–6.1 | Range |
| Ti | 0.20 | Maximum |
| Other elements, each | 0.05 | Maximum |
| Other elements, total | 0.15 | Maximum |
| Al | Remainder | Balance |
Registered AA limits, not nominal chemistry or certified heat analysis. Ranges show minimum–maximum; other numerical entries are maxima. Other-element provisions apply. No EN/producer chemistry is merged into these limits. Unlisted elements are not represented as zero or unrestricted; 7020 has a combined Zr+Ti limit rather than an invented separate Ti maximum. Confirm governing specification and heat certificate.
The Aluminum Association — Teal Sheets, December 2025
| Property | SI value | Condition / temperature |
|---|---|---|
| Density | ≈2796 kg/m³ | Nominal source 0.101 lb/in³; temperature and temper unspecified; direct unit conversion |
| Linear expansion | 23.58 × 10⁻⁶ K⁻¹ | Mean 20–100 °C; source 13.1 × 10⁻⁶ °F⁻¹ multiplied by 1.8; temper unspecified |
Alcoa cold-finished product sheet. Nominal reference data, not acceptance limits; not extrapolated to other temperatures.
T6 — bare sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / bare | 0.203–6.32 | 510–538 | 434–476 | 5–8 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T6 — alclad sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / alclad | 0.203–6.32 | 469–524 | 400–448 | 5–9 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T651 — bare plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / bare | 6.35–101.60 | 538–462 | 462–372 | 9–3 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T651 — alclad plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / alclad | 6.35–101.60 | 517–462 | 448–372 | 9–3 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T73 — bare sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / bare | 1.02–6.32 | 462 | 386 | 8 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T73 — alclad sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / alclad | 1.02–6.32 | 434–455 | 352–372 | 8 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T7351 — bare plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / bare | 6.35–101.60 | 476–421 | 393–331 | 7–6 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T7351 — alclad plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / alclad | 6.35–25.40 | 455–476 | 372–393 | 8–7 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T76 — bare sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / bare | 3.18–6.32 | 503 | 427 | 8 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T76 — alclad sheet
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Sheet / alclad | 3.18–6.32 | 469–482 | 393–407 | 8 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T7651 — bare plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / bare | 6.35–25.40 | 496–490 | 421–414 | 8–6 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
T7651 — alclad plate
| Product / surface | Thickness (mm unless stated) | UTS (MPa unless stated) | Yield (MPa unless stated) | Elongation (%) | Orientation / basis |
|---|---|---|---|---|---|
| Plate / alclad | 6.35–25.40 | 476–490 | 400–414 | 8–6 | LT; minima across reported gauge range |
Test temperature and elongation gauge length not stated. Ranges are producer summaries of thickness-dependent minima, NOT typical values or a single guaranteed minimum at every thickness; intermediate thickness sub-bands are not supplied. Do not interpolate. Bare and alclad data are independent.
Solution treatment and quenching
Dissolve soluble phases and quench to retain supersaturation. Control transfer, cooling uniformity and distortion with a qualified product-specific procedure; thick sections cannot be assigned thin-sheet response.
Artificial ageing
T6 develops high strength by artificial ageing after solution treatment; T651 additionally identifies stretching stress relief for the documented plate product.
Overageing
T73/T7351 favour SCC resistance; T76/T7651 favour exfoliation resistance at a different strength balance. These conditions are not equivalent to T6/T651 or to one another.
Stress relief and machining
The 51 suffix identifies stretching stress relief; it does not guarantee freedom from residual stress or distortion. Plan balanced roughing and finishing around section removal.
Forming and re-treatment
Forming in softer O or solution-treated W condition may be appropriate only under qualified handling and re-treatment procedures. Do not improvise ageing or solution-treatment schedules.
Conceptual guidance only: no furnace temperatures, soak times, quench delays or ageing schedules are supplied. Product-specific procedures and final temper must be qualified.
Material selection
Corrosion resistance & performance
General corrosion resistance requires protective-system selection; avoid galvanic contact and protect joints, machined edges and faying surfaces. Alcladding is not proof against every corrosion mode.
Alcoa identifies T76-type tempers as exfoliation resistant and T73-type tempers as SCC resistant. T73 also resists exfoliation at lower strength than T76; T6/T651 should not be assigned T73 performance.
Sustained tensile stress, residual stress, environment, orientation and section thickness govern SCC risk. No universal safe-stress threshold is asserted.
Typical applications
Engineering applications
- Aircraft skin sheet (including alclad products)
- Aerospace structural plate components
- Aircraft fittings
- Gears and shafts
- Highly stressed machined aerospace components
Subsequent manufacturing
Machining & processing
Machining
Good machinability is documented for heat-treated products. Use controlled stock removal, rigid support and suitable chip control; stress-relieved plate can still move during machining.
Forming
Heat-treated material has restricted cold formability. Confirm bend radius, direction and any softer-condition forming route with the producer; re-treatment changes the final condition.
Joining
Do not specify conventional fusion welding as a routine structural joining route for these high-strength Al–Zn–Mg–Cu products. Cracking sensitivity, heat-affected-zone strength loss and corrosion changes require application-specific qualification. Resistance or solid-state joining is a separate qualified process, not blanket approval for fusion welding.
Damage tolerance
7075 provides a baseline strength/toughness balance. Reviewed typical toughness values lack a thickness basis, so no numerical toughness is assigned here. Select a damage-tolerant alternative or additional testing where required.
Material certification & testing
Certification is conditional on the agreed product specification, mill route and purchase order; no blanket aerospace approval or stock certification is implied.
No certificate or test is automatically included. Alloy designation alone does not establish aerospace drawing compliance: confirm specification/revision, temper, product form, thickness, test orientation and acceptance requirements.
- Request heat/lot traceability and chemical analysis.
- Agree temper, thickness band, surface/cladding, orientation, tensile acceptance and elongation basis.
- Specify any ultrasonic inspection, SCC/exfoliation, conductivity or residual-stress requirements before ordering.
- Agree fracture toughness method, specimen geometry, orientation, thickness and guaranteed limits where required; do not infer them from typical data.
- EN 10204 3.1 material certificate and Certificate of Conformity where agreed
- Temper verification, heat-treatment records and hardness testing where specified
- Customer-specific chemical/mechanical testing and aerospace inspection requirements where agreed
Material enquiry
Request a material quotation
Aluminium Alloy 7075 supplied to your material form, dimensions and specification.