Representative turned martensitic stainless steel round bars

Materials Supply / Stainless Steels

420 Stainless Steel

Martensitic Stainless Steel | AISI 420 | UNS S42000

Higher-carbon chromium martensitic stainless steel for hardened wear parts; carbon range and hardening response depend on the selected product.

Mechanical properties depend on supply condition, heat treatment and section size. The independently labelled condition tables are reference data, not guaranteed Quest Engineering supply properties.

Raw & semi-finished materials

Available material forms

Potential forms only, subject to supplier confirmation, dimensions, condition and the agreed product specification; no held stock or universal availability is claimed.

  • Round Bar
  • Flat Bar
  • Plate
  • Sheet
  • Cut-to-Size Material

Material overview

420 Stainless Steel

Higher-carbon chromium martensitic stainless steel for hardened wear parts; carbon range and hardening response depend on the selected product.

  • Higher-carbon chromium martensitic stainless steel for hardened wear parts; carbon range and hardening response depend on the selected product.
  • Magnetic martensitic grade; hardening and tempering alter strength, hardness and ductility.
  • Select the product form, chemistry and heat-treatment condition together; reference values must not be transferred between conditions.

Material specifications & designations

Material specifications & designations
DesignationReference
AISI420
UNSS42000
EN reference — grade-dependentNo single EN equivalent assigned. EN 420-family variants have different carbon ranges; identify the exact chemistry and standard before substitution.
ASTM A276Type 420 stainless steel bars and shapes; confirm ordered condition and edition
Flat productsATI producer plate, sheet, strip and flat-bar reference; exact ASTM/EN flat-product acceptance specification requires confirmation

UNS and EN references are comparison identifiers, not exact contractual equivalence. Current full ASTM, EN and AMS standards were not available for revision-specific verification. No A479, A182 or unverified blanket AMS equivalence is asserted. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • designations / product forms

    Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.

    Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.

  • mechanical / physical / certification

    Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.

    Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.

Engineering reference

Technical data

Chemical composition
ElementMinimum %Maximum %
Carbon0.150.40
Chromium12.014.0
Nickel—0.75
Manganese—1.00
Silicon—1.00
Phosphorus—0.040
Sulphur—0.030
IronBalanceBalance

ATI 420 producer flat-product chemistry, page 2 (2014): carbon 0.15–0.40%. Generic ASTM 420 references may specify a carbon minimum without this upper limit; 420HC is a separate variant. The condition samples explicitly state their own nominal carbon contents. Values are mass percentages (wt. %). A dash means no limit stated on that side, not zero. Do not combine this basis with another product-form specification.

Physical properties
PropertyIndicative valueCondition
Density≈ 7.73 g/cm³Nominal ambient; annealed (from specific gravity)
Elastic modulus≈ 200 GPaNominal ambient; exact test temperature not stated
Thermal conductivity≈ 24.2 W/(m·K)At 100°C; annealed
Mean thermal expansion coefficient≈ 10.8 × 10⁻⁶/KMean over 20–200°C; annealed
Electrical resistivity≈ 560 nΩ·mAt 20°C; annealed

Typical indicative values, not specification limits or design guarantees. Nominal ambient values lack an exact measurement temperature in the source. Resistivity is omitted where its test temperature is unsupported.

Annealed — sheet sample

Mechanical properties — Annealed — sheet sample
PropertyReference valueBasis
Ultimate tensile strength592 MPaTypical reference
0.2% proof strength355 MPaTypical reference
Hardness85 HRBTypical reference

ATI sheet sample reference (nominal 0.25% carbon), page 3. Typical values, not specification acceptance limits. Test temperature and specimen thickness are not stated. Do not apply automatically to bars or other section sizes. Elongation and impact values are not reported for this sample series and are omitted.

Hardened + tempered at 204°C — sheet sample

Mechanical properties — Hardened + tempered at 204°C — sheet sample
PropertyReference valueBasis
Ultimate tensile strength1759 MPaTypical reference
0.2% proof strength1311 MPaTypical reference
Hardness48 HRCTypical reference

ATI sheet sample reference (nominal 0.25% carbon), page 3. Typical values, not specification acceptance limits. Test temperature and specimen thickness are not stated. Do not apply automatically to bars or other section sizes. Elongation and impact values are not reported for this sample series and are omitted. This series was heated at 1038°C for 60 minutes per inch of thickness, air cooled to room temperature, then tempered at 204°C for two hours. The adjacent general discussion mentions oil quenching; the page 3 sample-specific air-cooling basis is used here. This is a laboratory reference, not a production schedule.

Annealing

ATI page 5 guidance for 420 flat products: 843–899°C, hold for one hour per inch of thickness, then furnace cool to room temperature. This producer reference cycle requires section- and application-specific confirmation; it is not a universal 420 production schedule.

Hardening and tempering

The displayed ATI sheet example with nominal 0.25% C was hardened at 1038°C, air cooled, then tempered at 204°C for two hours. It is a sample-specific reference and must not be transferred to all 420 carbon variants or section sizes.

Processing limitations

420HC and other higher-carbon variants are distinct producer products. Quenching distortion, cracking and tempering-related toughness loss require a qualified cycle and finish-machining allowance.

General processing guidance and separately labelled producer examples only; not guaranteed material specifications or a qualified production schedule. Confirm furnace control, section size, atmosphere, cooling and acceptance tests with the supplier and heat treater.

Material selection

Corrosion resistance & performance

Corrosion resistance depends on heat treatment, surface finish, exposure and cleanliness. These martensitic grades are not substitutes for the general corrosion resistance of 316 in aggressive environments.

Hardened and appropriately tempered, clean polished surfaces generally perform best in mild atmospheric or compatible fresh-water exposure. General corrosion resistance is below common 304/316 austenitic grades.

No universal chemical compatibility, marine suitability or maximum service temperature is implied. Assess the actual application and subsequent tempering or thermal exposure.

Typical applications

Engineering applications

  • Cutlery and cutting edges
  • Surgical instruments to applicable requirements
  • Wear-resistant tooling
  • Valve seats and precision wear parts

Subsequent manufacturing

Machining & processing

Machinability

Annealed or suitably tempered stock is generally easier to machine than fully hardened stock. Specify incoming hardness and allow for the intended finishing process.

Deformation and work hardening

Cold deformation changes hardness and residual stress; these grades do not have the forming behaviour of annealed 304/316. Avoid assuming deep-drawing or extensive cold-forming capability.

Heat treatment and stability

Account for distortion, dimensional movement and cracking during quenching. Specify machining allowance, final condition and hardness checks; agree welding and post-weld treatment separately.

Surface finishing

Use a clean, suitable ground or polished finish and avoid iron contamination. Cleaning and any passivation process must suit the grade, heat treatment and service environment.

Material certification & testing

Documentation and testing may be requested, subject to supplier confirmation:

Confirm certificates, testing, product condition and acceptance criteria at quotation stage. No certification or testing is promised unless specifically agreed.

  • EN 10204 3.1 material certificates
  • Manufacturer Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical test reports
  • Hardness testing
  • Additional inspection or testing where applicable

Material enquiry

Request a material quotation

420 Stainless Steel supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.