Materials Supply / Stainless Steels
Nitronic 60 Stainless Steel
Nitrogen-Strengthened Austenitic Stainless Steel | UNS S21800
Austenitic stainless steel recognised for resistance to galling and adhesive wear in sliding and threaded assemblies.
Galling performance depends on the mating material, contact pressure, lubrication, temperature and surface finish. Wear resistance does not establish suitability for every bearing, sliding contact or corrosive environment.
NITRONIC® is a registered trademark of Cleveland-Cliffs Inc., as attributed in the cited producer bulletin.
Raw & semi-finished materials
Available material forms
Potential forms supported by producer references; size, material condition, availability and specification require supplier confirmation. No Quest Engineering stock holding or immediate availability is implied.
- Round Bar
- Wire
- Forging Billets
- Cut-to-Size Material
Material overview
Nitronic 60 Stainless Steel
Austenitic stainless steel recognised for resistance to galling and adhesive wear in sliding and threaded assemblies.
- Austenitic stainless steel recognised for resistance to galling and adhesive wear in sliding and threaded assemblies.
- Strengthening is achieved by nitrogen alloying and controlled deformation, not conventional martensitic precipitation-hardening treatments.
- Agree the exact product form, size, condition and test requirements; typical reference measurements are not guaranteed supply properties.
Material specifications & designations
| Designation | Reference |
|---|---|
| UNS | S21800 |
| Commercial designation | Nitronic 60 |
| ASTM A276 / A479 | Bars and shapes / bars and shapes for boiler and pressure-vessel construction, respectively; producer grade association |
| ASTM A314 | Stainless billets and bars intended only for forging; forging stock, not finished forgings |
| ASTM A580 | Stainless wire in coils; straightened/cut lengths are referred to A276 or A479 |
| ASTM A193 B8S / A194 8S | Producer-associated bolting materials/components / nuts for specified high-temperature or high-pressure applications; class and size must be agreed separately |
| AMS 5848 | Solution-heat-treated bars, wire, forgings, extrusions, mechanical tubing, flash-welded rings and associated stock; SAE public scope, not plate/sheet |
| EN reference | No verified EN material number or exact equivalent is asserted. |
Grade associations are producer-listed; public standard scopes are checked separately. Full current ASTM/AMS requirements were not available. Confirm grade, revision, product form, dimensions, condition and test requirements; no current-standard compliance or blanket aerospace approval is claimed. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.
Specification review
Technical verification requirements
designations / product forms
Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.
Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.
mechanical / physical / certification
Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.
Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.
Engineering reference
Technical data
| Element | Minimum mass % | Maximum mass % |
|---|---|---|
| Carbon | — | 0.10 |
| Chromium | 16.00 | 18.00 |
| Nickel | 8.00 | 9.00 |
| Manganese | 7.00 | 9.00 |
| Silicon | 3.50 | 4.50 |
| Nitrogen | 0.08 | 0.18 |
| Phosphorus | — | 0.040 |
| Sulphur | — | 0.030 |
| Iron | Balance | Balance |
One ARMCO producer composition basis, p. 1, in mass % (wt. %), not a current ASTM chemistry transcription or heat analysis. A dash means no minimum stated, not zero. Iron balance is an editorial remainder for this iron-base alloy; the producer does not tabulate iron. Electralloy nominal analysis lists sulphur ≤0.010%, unlike ARMCO ≤0.030%; that alternative is not blended into this table. Confirm the ordered standard and supplier heat analysis.
| Property | Indicative value | Condition / temperature |
|---|---|---|
| Density | ≈ 7,622 kg/m³ | At 24°C; p. 32 Table 50, condition not stated |
| Elastic modulus | ≈ 180 GPa | P. 32 Table 50; condition and test temperature not stated |
| Mean thermal expansion coefficient | ≈ 15.8 × 10⁻⁶/K | Mean 24–93°C; p. 32 Table 51, condition not stated |
| Electrical resistivity | ≈ 982 nΩ·m | P. 32 Table 50; temperature/condition not stated, converted from 98.2 μΩ·cm |
Typical informational values, not acceptance limits or design allowables. Conditions and temperatures are identified only where supplied; omitted source details are not assumed. Unit conversions use 1 μΩ·cm = 10 nΩ·m. The primary producer bulletin does not supply thermal conductivity; a temperature-qualified value requires further verification.
Annealed
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 710 MPa | Typical producer test value |
| 0.2% proof strength | 414 MPa | Typical producer test value |
| Elongation (4D₀) | 64% | Typical producer test value |
| Hardness | 95 HRB | Typical producer test value |
| Reduction of area | 74% | Typical producer test value |
March 2023 p. 3 Table 1, typical room-temperature annealed diameter 25.4 mm stock; duplicate tests, elongation in 4D₀. Numerical test temperature and orientation are not stated. Not the separate Table 7 bar/wire acceptance proposal or current ASTM minima.
10% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 827 MPa | Typical producer test value |
| 0.2% proof strength | 627 MPa | Typical producer test value |
| Elongation (4D₀) | 51% | Typical producer test value |
| Hardness | 24 HRC | Typical producer test value |
| Reduction of area | 68% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
20% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 965 MPa | Typical producer test value |
| 0.2% proof strength | 772 MPa | Typical producer test value |
| Elongation (4D₀) | 35% | Typical producer test value |
| Hardness | 31 HRC | Typical producer test value |
| Reduction of area | 65% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
30% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 1110 MPa | Typical producer test value |
| 0.2% proof strength | 910 MPa | Typical producer test value |
| Elongation (4D₀) | 26% | Typical producer test value |
| Hardness | 34 HRC | Typical producer test value |
| Reduction of area | 62% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
40% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 1344 MPa | Typical producer test value |
| 0.2% proof strength | 1055 MPa | Typical producer test value |
| Elongation (4D₀) | 20% | Typical producer test value |
| Hardness | 38 HRC | Typical producer test value |
| Reduction of area | 57% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
50% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 1496 MPa | Typical producer test value |
| 0.2% proof strength | 1200 MPa | Typical producer test value |
| Elongation (4D₀) | 15% | Typical producer test value |
| Hardness | 41 HRC | Typical producer test value |
| Reduction of area | 53% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
60% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 1655 MPa | Typical producer test value |
| 0.2% proof strength | 1344 MPa | Typical producer test value |
| Elongation (4D₀) | 12% | Typical producer test value |
| Hardness | 43 HRC | Typical producer test value |
| Reduction of area | 48% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
70% Cold Drawn
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 1813 MPa | Typical producer test value |
| 0.2% proof strength | 1496 MPa | Typical producer test value |
| Elongation (4D₀) | 10% | Typical producer test value |
| Hardness | 46 HRC | Typical producer test value |
| Reduction of area | 40% | Typical producer test value |
March 2023 p. 3 Table 1: typical room-temperature cold-drawn round-stock test values, 11.2 mm starting diameter (not final diameter), duplicate tests and elongation in 4D₀. Exact numeric temperature, finished section and orientation are not stated. The percentage is the producer-labelled cold-drawn reduction; these rows are not the separately hot-worked HS bar condition or guaranteed supply minima.
Solution annealing
The March 2023 producer bulletin recommends annealing at 1066°C followed by water quenching. No soak duration is given. This austenitic alloy is not hardened by conventional heat treatment or PH ageing.
Cold work and separate HS bar
Cold drawing develops the condition-dependent strength shown in Table 1, with reduced ductility. Producer HS bar is a separate hot-worked unannealed offering, not a synonym for these cold-drawn conditions. Welding, hot forging or solution annealing can remove processing-derived strength; aqueous corrosion resistance may also change.
Grade-specific producer guidance only, not a qualified manufacturing schedule. Confirm section size, furnace controls, soak, cooling and required final tests against the ordered product specification.
Material selection
Corrosion resistance & performance
Resistance to galling and adhesive wear is the main selection characteristic, particularly for sliding contact and threaded assemblies. Contact stress, mating materials, lubrication, finish, temperature and wear mode must be assessed; no universal bearing suitability or wear allowable is implied.
General corrosion and chloride-pitting behaviour are different criteria. Producer sources describe general corrosion between 304 and 316 while selected pitting tests outperform 316. Do not assume immunity to chlorides, crevice attack or stress-corrosion cracking, or universal superiority to 316.
Typical applications
Engineering applications
- Valve stems, seats and trim
- Bushings and pins
- Fasteners and thread inserts
- Pump wear rings and lobes
- Sliding and threaded assemblies
- Wear-resistant mechanical parts subject to engineering assessment
Subsequent manufacturing
Machining & processing
Machinability
Use austenitic-stainless machining practice with sharp tooling, sustained cuts and appropriate coolant. Nitrogen strengthening and processing-derived hardness increase tool loads; avoid rubbing or dwelling. Producer tool-life examples are not universal cutting-speed factors.
Work hardening and forming
Cold deformation increases strength and reduces ductility. Match stock condition to forming requirements and allow for residual stress or any necessary intermediate annealing.
Welding
The producer describes conventional welding methods. Select qualified procedures and suitable filler for corrosion and mechanical requirements; welds can lose the strengthening of HS or cold-worked stock. Weld deposits and overlays have separately evaluated wear characteristics, not automatic base-metal galling performance.
Surface finishing
Agree surface finish and cleanliness for the service. Avoid embedded carbon-steel contamination, remove weld/heat-treatment scale where required and qualify cleaning or passivation; surface finish affects corrosion and sliding-contact behaviour.
Material certification & testing
Documentation and testing may be requested subject to customer requirements and supplier confirmation:
Agree the ordered specification, revision, material condition and acceptance criteria before supply. Certification or aerospace conformity is not promised without matching supplier documents.
- EN 10204 3.1 material certificates
- Manufacturer Certificates of Conformity
- Heat/batch traceability
- Chemical analysis
- Mechanical testing
- Positive Material Identification (PMI)
- Additional testing where applicable
Material enquiry
Request a material quotation
Nitronic 60 Stainless Steel supplied to your material form, dimensions and specification.