Representative precipitation-hardening stainless steel round bars

Materials Supply / Stainless Steels

15-5PH Stainless Steel

Martensitic Precipitation-Hardening Stainless Steel | UNS S15500

Chromium-nickel-copper martensitic precipitation-hardening stainless steel developed for improved transverse toughness relative to 17-4PH.

Supply condition and ageing determine the balance of strength, hardness and toughness. Condition-specific reference data must not be transferred between bar, plate, strip or forgings.

Raw & semi-finished materials

Available material forms

Potential forms supported by the cited producer/specification references; dimensions, supply condition, availability and certification must be confirmed. No Quest Engineering stock holding is implied.

  • Round Bar
  • Flat Bar
  • Plate
  • Forgings
  • Cut-to-Size Material

Material overview

15-5PH Stainless Steel

Chromium-nickel-copper martensitic precipitation-hardening stainless steel developed for improved transverse toughness relative to 17-4PH.

  • Chromium-nickel-copper martensitic precipitation-hardening stainless steel developed for improved transverse toughness relative to 17-4PH.
  • Copper-containing precipitates strengthen the martensitic matrix.
  • Verify the ordered product specification, ageing condition, size and test requirements for the application.

Material specifications & designations

Material specifications & designations
DesignationReference
UNSS15500
Common designation15-5PH
AMS 5659Bars, wire, forgings, flash-welded rings and extrusions; solution heat treated. SAE scope and Hillfoot Rev T reference; aged slash conditions require separate confirmation.
AMS 5862Sheet, strip and plate — historical producer association; confirm the ordered AMS 5862 revision, nominal thickness, melt route and delivery condition. Not a bar or forging specification.
ASTM A564 / A693 / A705Respectively bars/wire/shapes; sheet/plate/strip; forgings — product-specific requirements
EN referenceNo EN material number asserted: exact chemistry, product-form standard and contractual equivalence require separate verification.

Specification applicability follows product form and condition, not similar chemistry. Public scope/producer listings were checked, but current full AMS/ASTM/EN acceptance tables were unavailable. Confirm the purchased revision and any slash-condition designation; no aerospace conformity is promised without matching certificates.

Specification review

Technical verification requirements

  • designations / product forms

    Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.

    Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.

  • mechanical / physical / certification

    Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.

    Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.

  • heatTreatment

    Overview intentionally omits some hold times/cooling/transition details. It must not function as a complete production route; semi-austenitic TH/RH/CH precursors in particular are not interchangeable. No exact numerical error is asserted where missing parameters are expressly deferred.

    Have heat-treatment authority specify full applicable grade/form cycle, atmosphere, tolerances, transfer times, cooling and final acceptance tests; retain overview disclaimer.

Engineering reference

Technical data

Chemical composition — historical producer reference
ElementProducer-reported wt. %
Carbon0.07 max.
Manganese1.00 max.
Phosphorus0.04 max.
Sulfur0.03 max.
Silicon1.00 max.
Chromium14.00–15.00
Nickel3.50–5.50
Copper2.50–4.50
Niobium (columbium) + tantalum0.15–0.45
IronBalance

Historical Carpenter 15Cr-5Ni Stainless (UNS S15500) producer reference, 2009 Guide, printed p. 13. The entry explicitly states single figures are maximums; paired figures are reproduced as ranges, not converted to nominal point values. This is not verified current ASTM A564 or AMS chemistry and is not an acceptance table for Quest supply. The chromium range is reproduced exactly as 14.00–15.00, not silently changed to 15.50. Confirm the ordered specification and revision before purchasing; if a historical producer reference is unsuitable, omit this table rather than substitute unverified standard limits.

Physical properties
PropertyIndicative valueCondition / temperature
Density≈ 7.75 g/cm³Condition A; nominal ambient, exact temperature unstated
Density≈ 7.81 g/cm³H900; nominal ambient
Density≈ 7.83 g/cm³H1075; nominal ambient
Density≈ 7.86 g/cm³H1150; nominal ambient
Elastic modulus≈ 196 GPaA / H900 / H1075 / H1150; nominal ambient
Thermal conductivity≈ 18.3 W/(m·K)Condition A; source reports 21–100°C interval
Thermal conductivity≈ 17.8 W/(m·K)H900; source reports 21–100°C interval
Mean thermal expansion coefficient≈ 11.3 × 10⁻⁶/KCondition A; mean 21–427°C
Mean thermal expansion coefficient≈ 11.7 × 10⁻⁶/KH900; mean 21–427°C

Typical producer values, not acceptance limits or design allowables. Conditions and temperature intervals are stated wherever supplied; nominal ambient means exact temperature is not identified. Unsupported graph estimates and resistivity without test temperatures are omitted.

Condition A

Mechanical properties — Condition A
PropertyReference valueBasis
Ultimate tensile strength1030 MPaTypical producer reference
0.2% proof strength760 MPaTypical producer reference
Elongation (50.8 mm)8%Typical producer reference
Hardness33 HRCTypical producer reference

ATI p. 4 typical room-temperature tensile table for the producer flat-product reference. Specimen thickness and orientation are not stated. These are not ASTM/AMS acceptance limits and must not be transferred to bar or forgings. The four conditions shown have directly readable producer values; other conditions require separate data.

H900

Mechanical properties — H900
PropertyReference valueBasis
Ultimate tensile strength1340 MPaTypical producer reference
0.2% proof strength1200 MPaTypical producer reference
Elongation (50.8 mm)15%Typical producer reference
Hardness43 HRCTypical producer reference

ATI p. 4 typical room-temperature tensile table for the producer flat-product reference. Specimen thickness and orientation are not stated. These are not ASTM/AMS acceptance limits and must not be transferred to bar or forgings. The four conditions shown have directly readable producer values; other conditions require separate data.

H1075

Mechanical properties — H1075
PropertyReference valueBasis
Ultimate tensile strength1070 MPaTypical producer reference
0.2% proof strength930 MPaTypical producer reference
Elongation (50.8 mm)15%Typical producer reference
Hardness36 HRCTypical producer reference

ATI p. 4 typical room-temperature tensile table for the producer flat-product reference. Specimen thickness and orientation are not stated. These are not ASTM/AMS acceptance limits and must not be transferred to bar or forgings. The four conditions shown have directly readable producer values; other conditions require separate data.

H1150

Mechanical properties — H1150
PropertyReference valueBasis
Ultimate tensile strength1000 MPaTypical producer reference
0.2% proof strength860 MPaTypical producer reference
Elongation (50.8 mm)15%Typical producer reference
Hardness31 HRCTypical producer reference

ATI p. 4 typical room-temperature tensile table for the producer flat-product reference. Specimen thickness and orientation are not stated. These are not ASTM/AMS acceptance limits and must not be transferred to bar or forgings. The four conditions shown have directly readable producer values; other conditions require separate data.

Solution treatment

ATI flat-product Condition A: approximately 1040–1065°C and cool to room temperature. No soak time or guaranteed dimensional limit is invented.

Ageing

H900, H1075 and H1150 are confirmed by the ATI typical property table. Their condition names identify nominal 482°C, 579°C and 621°C ageing treatments, respectively. Exact hold times and cooling must be agreed against the product specification; no schedule is copied from 17-4PH.

Condition and form

Reduced delta-ferrite content and processing support improved transverse toughness, but no guaranteed transverse or fracture toughness is claimed for every product form. H1025 properties require a separately confirmed reference.

Grade-specific producer processing guidance, not a qualified production schedule or guaranteed acceptance specification. Confirm furnace control, precursor condition, section size, hold times, cooling and tests to the ordered standard. Do not use this overview as a furnace work instruction or select a production route from conflicting source examples. A materials/process authority must approve the complete form- and condition-specific cycle, including precursor condition, section size, hold times, cooling and verification tests.

Material selection

Corrosion resistance & performance

General corrosion behaviour is broadly comparable to 17-4PH, with condition-dependent stress-corrosion performance. Improved toughness does not mean universally improved chemical resistance.

Assess medium, temperature, applied stress, crevices, surface finish and heat-treatment history. Remove contamination and heat-treatment scale; no marine suitability or maximum service temperature is implied.

Typical applications

Engineering applications

  • Structural fittings and fasteners
  • Actuator components
  • Shafts and gears
  • Aerospace parts requiring specified transverse properties

Subsequent manufacturing

Machining & processing

Machinability

Machine in solution-treated or separately specified overaged stock where appropriate. Ageing increases hardness and cutting forces; do not transfer strip data to bar machining.

Work hardening and forming

Cold work changes residual stress and subsequent ageing response. Specify incoming condition and any intermediate solution treatment with the producer.

Heat treatment and dimensional stability

Ageing can change dimensions and surface condition; retain appropriate allowance and qualify the full cycle for the product geometry. Low-temperature ageing does not guarantee zero distortion.

Welding and finishing

Use a qualified welding procedure, suitable filler and agreed post-weld heat treatment; matching strength and toughness require specification-specific assessment. Finish and clean surfaces with a grade-appropriate process; avoid embedded carbon-steel contamination.

Material certification & testing

Documentation and testing may be requested subject to supplier and quotation confirmation:

For aerospace orders, certificates must demonstrate conformity to the actual ordered specification, product form and material condition. Tests, traceability and acceptance criteria must be agreed at quotation; no certification is promised in advance.

  • EN 10204 3.1 material certificates
  • Manufacturer Certificates of Conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical test reports
  • Hardness testing
  • Heat-treatment records
  • Additional testing where required

Material enquiry

Request a material quotation

15-5PH Stainless Steel supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.