Materials Supply / Stainless Steels
304L Stainless Steel
Austenitic Stainless Steel | AISI 304L | UNS S30403 | EN 1.4307
304L is the low-carbon variant of 304, with carbon limited to 0.030% in the cited flat-product reference. Its chromium-nickel austenitic structure combines good general corrosion resistance with high ductility.
Reduced carbon limits chromium carbide precipitation during welding and lowers the risk of associated intergranular corrosion. It does not improve chloride pitting resistance relative to 304.
304L is commonly selected for welded tanks, processing vessels and pipework. Its annealed ASTM flat-product strength minimums are lower than those for 304; high-temperature or pressure duty needs a separate design assessment.
Raw & semi-finished materials
Available material forms
Potential supply forms are subject to supplier availability, size, product specification and quotation confirmation; this is not a statement of held stock.
- Round Bar
- Flat Bar
- Plate
- Sheet
- Seamless Tube
- Hollow Bar
- Forgings
- Cut-to-Size Material
Material overview
304L Stainless Steel
Low-carbon chromium-nickel austenitic stainless steel for raw and semi-finished engineering material supply.
- Maximum carbon 0.030% in the cited ASTM A240/A240M reference.
- Good ductility and toughness in the annealed condition.
- Reduced weld-related sensitisation; qualified procedures and surface cleaning still matter.
- Cold working increases strength and hardness and can introduce magnetism.
Material specifications & designations
| Designation | Reference |
|---|---|
| AISI | 304L |
| UNS | S30403 |
| EN Material Number | 1.4307 |
| EN Steel Name | X2CrNi18-9 |
| ASTM A276 | Type 304L stainless steel bars and shapes |
| ASTM A479 | Type 304L bars for pressure applications |
| ASTM A240 | Type 304L plate, sheet and strip |
| ASTM A182 | F304L forged flanges, fittings, valves and parts; not a general sheet or bar specification |
| ASTM A312 | TP304L austenitic stainless steel pipe; tube must have its own agreed product specification |
| EN 10088-2 / EN 10088-3 | Part 2: sheet/plate/strip; Part 3: semi-finished products, bars, rods, wire, sections and bright products for general purposes |
| AMS 5647 | 304L bars and applicable forging products; solution heat treated, precise scope and revision to be agreed Supplier-listed grade/form association, not independently verified current revision acceptance requirements. |
| AMS 5511 | 304L sheet, strip and plate; solution heat treated |
Confirm the purchased standard revision, product form, dimensions and supply condition at quotation stage. EN and UNS comparisons are not contractual equivalence; specifications are not interchangeable. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.
Specification review
Technical verification requirements
designations / product forms
Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.
Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.
mechanical / physical / certification
Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.
Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.
Engineering reference
Technical data
| Element | Minimum % | Maximum % |
|---|---|---|
| Carbon | — | 0.030 |
| Chromium | 18.0 | 20.0 |
| Nickel | 8.0 | 12.0 |
| Manganese | — | 2.0 |
| Silicon | — | 0.75 |
| Phosphorus | — | 0.045 |
| Sulphur | — | 0.030 |
| Nitrogen | — | 0.10 |
| Iron | Balance | Balance |
Main composition basis: ASTM A240/A240M-25a, Table 1, 304L Stainless Steel / S30403, plate, sheet and strip. Values are mass percentages (wt. %); a dash means no minimum specified, and iron is the balance. This is one dated flat-product specification basis, not bar, pipe, forging, EN or AMS chemistry. Verify the edition required by the purchase order and material certificate; ASTM lists A240/A240M-26 as active; its full requirement tables have not been verified in this review. The selected June 2025 edition is not claimed to be the latest.
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 485 MPa min. | Specification minimum |
| 0.2% proof strength | 170 MPa min. | Specification minimum |
| Elongation (50 mm) | 40% min. | Specification minimum |
| Hardness | 201 HBW max. | Specification maximum |
ASTM A240/A240M-25a, Table 2: room-temperature specification limits for annealed plate, sheet and strip, subject to A480/A480M general requirements. These are minimum strength/elongation and maximum hardness limits, not typical measurements or guaranteed Quest properties. Table 2 permits the designated Brinell or Rockwell test; only Brinell limits are shown here. Do not transfer these values to bar, pipe, forgings or AMS supply. Confirm the purchased edition, dimensions and condition; the active A240/A240M-26 tables were not independently verified.
| Property | Indicative value | Condition |
|---|---|---|
| Density | ≈ 7,900 kg/m³ | Nominal ambient; annealed |
| Elastic modulus | ≈ 193 GPa | Nominal ambient; annealed |
| Thermal conductivity | ≈ 16.3 W/(m·K) | At 100°C; annealed |
| Mean thermal expansion coefficient | ≈ 17.2 × 10⁻⁶/K | Mean over 0–100°C; annealed |
Typical annealed reference values, not specification acceptance limits or design guarantees. Density and modulus are nominal ambient reference values; the cited source does not give their exact measurement temperature. Thermal-property temperatures are shown explicitly. Confirm temperature-dependent design data for the application. Electrical resistivity is omitted because this reference does not identify its test temperature.
Material selection
Corrosion resistance & performance
Good general atmospheric corrosion resistance; assess chemical concentration, temperature, cleanliness and surface finish.
Chlorides may cause pitting, crevice corrosion and stress-corrosion cracking. Neither 304 nor 304L is a universal seawater or marine-service material.
Low carbon reduces sensitisation after welding, but does not eliminate corrosion risks from unsuitable processing or prolonged service.
Oxidation resistance does not establish an allowable service temperature. For elevated-temperature loads, verify creep, strength, sensitisation and cyclic exposure; the H-grade requirements are not interchangeable with this grade.
Typical applications
Engineering applications
- Welded chemical-processing vessels
- Food and pharmaceutical processing equipment
- Heat-exchanger fabrications
- Industrial pipework
- Welded tanks and containers
- Pumps and valve fabrications
- Instrumentation housings
- General fabricated engineering parts
Subsequent manufacturing
Machining & processing
Machinability
304L is not a free-machining grade. Use sharp tools, positive cutting action, adequate feeds and coolant; improved-machining stock requires a separate specification.
Work hardening
Avoid rubbing cuts and tool dwell. Cold deformation raises strength and hardness; machining plans must account for the stock condition.
Formability
Good ductility supports bending, rolling and drawing. Severe forming may require an agreed intermediate anneal.
Welding
Low carbon generally removes the need for post-weld annealing solely to control weld sensitisation. Select a qualified procedure and suitable low-carbon filler; other duty requirements may still require treatment.
Heat treatment
Cannot be hardened by conventional quench-and-temper treatment. Solution annealing and rapid cooling can restore ductility; agree the cycle to the specification and product dimensions.
Surface finishing
Grinding, polishing, pickling and passivation may be specified. Avoid carbon-steel contamination and remove weld heat tint using a suitable process.
Material certification & testing
Material may be supplied with documentation and testing according to customer requirements, including:
All documentation and additional testing are subject to quotation and confirmation. Specify the required certificates, tests and acceptance criteria; no approval or testing capability is implied.
- EN 10204 3.1 material test certificates
- Manufacturer certificates of conformity
- Heat/batch traceability
- Chemical analysis
- Mechanical test reports
- Positive Material Identification (PMI)
- Ultrasonic testing where applicable
Material enquiry
Request a material quotation