Materials Supply / Stainless Steels
347 Stainless Steel
Austenitic Stainless Steel | AISI 347 | UNS S34700 | EN 1.4550
347 is a niobium-stabilised chromium-nickel austenitic stainless steel. Niobium (also called columbium), with tantalum where present, binds carbon and helps reduce chromium carbide precipitation and associated intergranular corrosion.
It is used for welded process equipment, heat exchangers and exhaust components where post-weld annealing is impractical or prolonged thermal exposure makes a stabilised grade appropriate.
Stabilisation is not immunity to corrosion or an unlimited service-temperature rating. Chloride exposure, creep loads, weld condition and prolonged phase instability must be assessed for the duty; the higher-carbon H variant is a separate specification.
Raw & semi-finished materials
Available material forms
Potential supply forms are subject to supplier availability, size, product specification and quotation confirmation; this is not a statement of held stock.
- Round Bar
- Flat Bar
- Plate
- Sheet
- Seamless Tube
- Hollow Bar
- Forgings
- Cut-to-Size Material
Material overview
347 Stainless Steel
Niobium-stabilised chromium-nickel austenitic stainless steel for welded and elevated-temperature engineering applications.
- Niobium minimum is formula-based: 10 × actual carbon, maximum 1.00%, for ASTM A240/A240M-25a flat products.
- Good ductility and toughness in the annealed condition.
- General aqueous corrosion resistance is broadly comparable with 304, not the molybdenum-bearing 316 family.
- Stabilised chemistry supports resistance to sensitisation; severe duty may require an agreed stabilising heat treatment.
Material specifications & designations
| Designation | Reference |
|---|---|
| AISI | 347 |
| UNS | S34700 |
| EN Material Number | 1.4550 |
| EN Steel Name | X6CrNiNb18-10 |
| ASTM A276 | Type 347 stainless steel bars and shapes |
| ASTM A479 | Type 347 bars for pressure applications |
| ASTM A240 | Type 347 plate, sheet and strip |
| ASTM A182 | F347 forged flanges, fittings, valves and parts; not a general sheet or bar specification |
| ASTM A312 | TP347 austenitic stainless steel pipe; tube must have its own agreed product specification |
| EN 10088-2 / EN 10088-3 | Part 2: sheet/plate/strip; Part 3: semi-finished products, bars, rods, wire, sections and bright products for general purposes |
| AMS 5646 | 347 bars and applicable forging products; solution heat treated, precise scope and revision to be agreed |
| AMS 5512 | 347 sheet, strip and plate; solution heat treated |
Confirm the purchased standard revision, product form, dimensions and supply condition at quotation stage. EN and UNS comparisons are not contractual equivalence; specifications are not interchangeable. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.
Specification review
Technical verification requirements
designations / product forms
Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.
Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.
mechanical / physical / certification
Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.
Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.
Engineering reference
Technical data
| Element | Minimum % | Maximum % |
|---|---|---|
| Carbon | — | 0.08 |
| Chromium | 17.0 | 19.0 |
| Nickel | 9.0 | 13.0 |
| Manganese | — | 2.0 |
| Silicon | — | 0.75 |
| Phosphorus | — | 0.045 |
| Sulphur | — | 0.030 |
| Niobium (Nb) | 10 × C | 1.00 |
| Iron | Balance | Balance |
Main composition basis: ASTM A240/A240M-25a, Table 1, 347 Stainless Steel / S34700, plate, sheet and strip. Values are mass percentages (wt. %); a dash means no minimum specified, and iron is the balance. This is one dated flat-product specification basis, not bar, pipe, forging, EN or AMS chemistry. Verify the edition required by the purchase order and material certificate; ASTM lists A240/A240M-26 as active; its full requirement tables have not been verified in this review. The selected June 2025 edition is not claimed to be the latest. Niobium minimum is 10 × actual carbon, maximum 1.00%; the formula does not include nitrogen. No nitrogen or separate tantalum limit is specified for S34700 in this table. The older ATI nickel range and combined Nb+Ta wording are not used.
| Property | Reference value | Basis |
|---|---|---|
| Ultimate tensile strength | 515 MPa min. | Specification minimum |
| 0.2% proof strength | 205 MPa min. | Specification minimum |
| Elongation (50 mm) | 40% min. | Specification minimum |
| Hardness | 201 HBW max. | Specification maximum |
ASTM A240/A240M-25a, Table 2: room-temperature specification limits for annealed plate, sheet and strip, subject to A480/A480M general requirements. These are minimum strength/elongation and maximum hardness limits, not typical measurements or guaranteed Quest properties. Table 2 permits the designated Brinell or Rockwell test; only Brinell limits are shown here. Do not transfer these values to bar, pipe, forgings or AMS supply. Confirm the purchased edition, dimensions and condition; the active A240/A240M-26 tables were not independently verified.
| Property | Indicative value | Condition |
|---|---|---|
| Density | ≈ 7,960 kg/m³ | Nominal ambient; annealed |
| Elastic modulus | ≈ 193 GPa | Nominal ambient; annealed |
| Thermal conductivity | ≈ 16.3 W/(m·K) | Reference over 20–100°C; annealed |
| Mean thermal expansion coefficient | ≈ 16.6 × 10⁻⁶/K | Mean over 20–100°C; annealed |
| Electrical resistivity | ≈ 720 nΩ·m | At 20°C; annealed |
Typical annealed reference values, not specification acceptance limits or design guarantees. Density and modulus are nominal ambient reference values; the cited source does not give their exact measurement temperature. Thermal-property temperatures are shown explicitly. Confirm temperature-dependent design data for the application. ATI explicitly applies the thermal-property table to 321, 347 and 348; density is grade-specific. Resistivity converted from 72 μΩ·cm. Atlas quotes different 321 conductivity/density values; this table uses ATI consistently.
Material selection
Corrosion resistance & performance
General atmospheric and aqueous corrosion resistance is broadly comparable to 304 in the annealed condition; verify concentration, temperature and surface condition.
Niobium stabilisation reduces chromium carbide formation and improves resistance to sensitisation-related intergranular corrosion. Stabilisation does not eliminate every severe-service corrosion risk.
Chloride pitting, crevice corrosion and stress-corrosion cracking remain possible. No universal seawater or marine suitability is implied.
Useful oxidation resistance and elevated-temperature properties do not alone establish a safe operating temperature. Creep, stress rupture, phase stability and subsequent aqueous corrosion require duty-specific assessment.
Prolonged elevated-temperature exposure may cause sigma-phase embrittlement; verify the grade, thermal history and whether an H variant is actually specified.
Typical applications
Engineering applications
- Aircraft exhaust collectors
- Exhaust manifolds
- Heat exchangers
- Heavy welded process equipment
- Boiler casings
- Cabin-heater components
- Furnace components
- Energy-equipment fabrications
Subsequent manufacturing
Machining & processing
Machinability
347 needs sharp tools, positive cutting action and effective cooling. Allow for stock condition; it is not a free-machining grade.
Work hardening
Avoid rubbing or dwelling cuts. Cold working increases hardness and may require an agreed annealing stage.
Formability
Good ductility supports bending and rolling. Plan the forming sequence and heat treatment to preserve the required properties.
Welding
Suitable niobium-stabilised filler and a qualified procedure are required. Control cleanliness, shielding and heat input; austenitic welds require attention to hot-cracking susceptibility.
Heat treatment
Not hardenable by conventional thermal treatment. Solution annealing and, for severe service, a separate stabilising treatment may be specified; agree cycles with the supplier and purchaser.
Surface finishing
Specify grinding, polishing, descaling or passivation as required. Remove weld heat tint appropriately and avoid carbon-steel contamination.
Material certification & testing
Material may be supplied with documentation and testing according to customer requirements, including:
All documentation and additional testing are subject to quotation and confirmation. Specify the required certificates, tests and acceptance criteria; no approval or testing capability is implied.
- EN 10204 3.1 material test certificates
- Manufacturer certificates of conformity
- Heat/batch traceability
- Chemical analysis
- Mechanical test reports
- Positive Material Identification (PMI)
- Ultrasonic testing where applicable
Material enquiry
Request a material quotation
347 Stainless Steel supplied to your material form, dimensions and specification.