Representative austenitic stainless steel round bars

Materials Supply / Stainless Steels

321 Stainless Steel

Austenitic Stainless Steel | AISI 321 | UNS S32100 | EN 1.4541

321 is a titanium-stabilised chromium-nickel austenitic stainless steel. Titanium binds carbon and helps preserve chromium in solid solution, reducing sensitisation-related intergranular corrosion after thermal exposure.

It combines good forming and welding characteristics with useful elevated-temperature strength. It is used for bellows, expansion joints, heat exchangers and furnace parts where thermal history and subsequent corrosion exposure matter.

Stabilisation is not immunity to corrosion or an unlimited service-temperature rating. Chloride exposure, creep loads, weld condition and prolonged phase instability must be assessed for the duty; the higher-carbon H variant is a separate specification.

Raw & semi-finished materials

Available material forms

Potential supply forms are subject to supplier availability, size, product specification and quotation confirmation; this is not a statement of held stock.

  • Round Bar
  • Flat Bar
  • Plate
  • Sheet
  • Seamless Tube
  • Hollow Bar
  • Forgings
  • Cut-to-Size Material

Material overview

321 Stainless Steel

Titanium-stabilised chromium-nickel austenitic stainless steel for welded and elevated-temperature engineering applications.

  • Titanium minimum is formula-based: 5 × (carbon + nitrogen) in the cited ASTM reference.
  • Good ductility and toughness in the annealed condition.
  • General aqueous corrosion resistance is broadly comparable with 304, not the molybdenum-bearing 316 family.
  • Stabilised chemistry supports resistance to sensitisation; severe duty may require an agreed stabilising heat treatment.

Material specifications & designations

Material specifications & designations
DesignationReference
AISI321
UNSS32100
EN Material Number1.4541
EN Steel NameX6CrNiTi18-10
ASTM A276Type 321 stainless steel bars and shapes
ASTM A479Type 321 bars for pressure applications
ASTM A240Type 321 plate, sheet and strip
ASTM A182F321 forged flanges, fittings, valves and parts; not a general sheet or bar specification
ASTM A312TP321 austenitic stainless steel pipe; tube must have its own agreed product specification
EN 10088-2 / EN 10088-3Part 2: sheet/plate/strip; Part 3: semi-finished products, bars, rods, wire, sections and bright products for general purposes
AMS 5645321 bars and applicable forging products; solution heat treated, precise scope and revision to be agreed
AMS 5510321 sheet, strip and plate; solution heat treated

Confirm the purchased standard revision, product form, dimensions and supply condition at quotation stage. EN and UNS comparisons are not contractual equivalence; specifications are not interchangeable. Reference associations only: no equivalence, stock availability, aerospace approval or certified conformity is established by this page. Specify the ordered revision, product form, dimensions, manufacture/melt route, delivery condition and acceptance tests; obtain matching supplier confirmation and inspection documents.

Specification review

Technical verification requirements

  • designations / product forms

    Public grade associations do not establish revision-specific acceptance for every listed standard and offered form. Each row remains subject to contractual form, grade, process and delivery-condition checking; pipe is not generic tube, forging stock is not a finished forging, and long-product AMS is not flat product approval. This is an evidence gap, not a finding that all listed mappings are wrong.

    Obtain ordered revisions; sign off each listed row against grade, form, size, melt route, condition and any slash designation; document offered tube specification separately where relevant.

  • mechanical / physical / certification

    Published reference data are not a Quest certified delivery envelope. Some tables explicitly lack orientation, specimen size or test temperature; preserve those caveats. Conditional certificate/PMI/UT availability is not evidence of actual supplier capability or aerospace approval.

    Retain typical-versus-minimum distinctions; confirm actual purchase-order test orientation, dimensions, temperature and certificate/test acceptance requirements before publication or supply.

Engineering reference

Technical data

Chemical composition
ElementMinimum %Maximum %
Carbon—0.08
Chromium17.019.0
Nickel9.012.0
Manganese—2.0
Silicon—0.75
Phosphorus—0.045
Sulphur—0.030
Nitrogen—0.10
Titanium5 × (C + N)0.70
IronBalanceBalance

Main composition basis: ASTM A240/A240M-25a, Table 1, 321 Stainless Steel / S32100, plate, sheet and strip. Values are mass percentages (wt. %); a dash means no minimum specified, and iron is the balance. This is one dated flat-product specification basis, not bar, pipe, forging, EN or AMS chemistry. Verify the edition required by the purchase order and material certificate; ASTM lists A240/A240M-26 as active; its full requirement tables have not been verified in this review. The selected June 2025 edition is not claimed to be the latest. Titanium minimum is 5 × (actual C + actual N), maximum 0.70%; do not use the different 321H stabiliser formula.

Mechanical properties
PropertyReference valueBasis
Ultimate tensile strength515 MPa min.Specification minimum
0.2% proof strength205 MPa min.Specification minimum
Elongation (50 mm)40% min.Specification minimum
Hardness217 HBW max.Specification maximum

ASTM A240/A240M-25a, Table 2: room-temperature specification limits for annealed plate, sheet and strip, subject to A480/A480M general requirements. These are minimum strength/elongation and maximum hardness limits, not typical measurements or guaranteed Quest properties. Table 2 permits the designated Brinell or Rockwell test; only Brinell limits are shown here. Do not transfer these values to bar, pipe, forgings or AMS supply. Confirm the purchased edition, dimensions and condition; the active A240/A240M-26 tables were not independently verified.

Physical properties
PropertyIndicative valueCondition
Density≈ 7,920 kg/m³Nominal ambient; annealed
Elastic modulus≈ 193 GPaNominal ambient; annealed
Thermal conductivity≈ 16.3 W/(m·K)Reference over 20–100°C; annealed
Mean thermal expansion coefficient≈ 16.6 × 10⁻⁶/KMean over 20–100°C; annealed
Electrical resistivity≈ 720 nΩ·mAt 20°C; annealed

Typical annealed reference values, not specification acceptance limits or design guarantees. Density and modulus are nominal ambient reference values; the cited source does not give their exact measurement temperature. Thermal-property temperatures are shown explicitly. Confirm temperature-dependent design data for the application. ATI explicitly applies the thermal-property table to 321, 347 and 348; density is grade-specific. Resistivity converted from 72 μΩ·cm. Atlas quotes different 321 conductivity/density values; this table uses ATI consistently.

Material selection

Corrosion resistance & performance

General atmospheric and aqueous corrosion resistance is broadly comparable to 304 in the annealed condition; verify concentration, temperature and surface condition.

Titanium stabilisation reduces chromium carbide formation and associated intergranular corrosion. Severe prolonged exposure and welding can still require an agreed stabilising treatment.

Chloride pitting, crevice corrosion and stress-corrosion cracking remain possible. No universal seawater or marine suitability is implied.

Useful oxidation resistance and elevated-temperature properties do not alone establish a safe operating temperature. Creep, stress rupture, phase stability and subsequent aqueous corrosion require duty-specific assessment.

Prolonged elevated-temperature exposure may cause sigma-phase embrittlement; verify the grade, thermal history and whether an H variant is actually specified.

Typical applications

Engineering applications

  • Expansion joints
  • Bellows
  • Furnace parts
  • Heating-element tubing
  • Heat exchangers
  • Burner pipes and flues
  • Aerospace exhaust components subject to specification
  • Elevated-temperature screens

Subsequent manufacturing

Machining & processing

Machinability

321 needs sharp tools, positive cutting action and effective cooling. Allow for stock condition; it is not a free-machining grade.

Work hardening

Avoid rubbing or dwelling cuts. Cold working increases hardness and may require an agreed annealing stage.

Formability

Good ductility supports bending and rolling. Plan the forming sequence and heat treatment to preserve the required properties.

Welding

Titanium can be lost across the arc; 347-type niobium-stabilised filler is commonly used for 321. Confirm the qualified procedure, shielding, cleanliness and duty requirements.

Heat treatment

Not hardenable by conventional thermal treatment. Solution annealing and, for severe service, a separate stabilising treatment may be specified; agree cycles with the supplier and purchaser.

Surface finishing

321 is less suited to a high decorative polish than some other austenitic grades. Specify the required finish, descaling and passivation; prevent iron contamination.

Material certification & testing

Material may be supplied with documentation and testing according to customer requirements, including:

All documentation and additional testing are subject to quotation and confirmation. Specify the required certificates, tests and acceptance criteria; no approval or testing capability is implied.

  • EN 10204 3.1 material test certificates
  • Manufacturer certificates of conformity
  • Heat/batch traceability
  • Chemical analysis
  • Mechanical test reports
  • Positive Material Identification (PMI)
  • Ultrasonic testing where applicable

Material enquiry

Request a material quotation

321 Stainless Steel supplied to your material form, dimensions and specification.

Material quotation requirements

Attachments — optional

PDF, STEP / STP, text DXF, supported DWG, XLSX, DOCX, JPG, PNG. For legacy DOC / XLS or binary DXF, please export to a supported format.

OR drag and drop files here

6.00 MB remaining of 6 MB

    Attachment limit: 6 MB combined

    If your engineering drawings exceed 6 MB, please submit your enquiry without attachments and we will contact you to arrange a suitable file transfer.

    Files are attached directly to your enquiry email. File validation is not malware scanning.